Erbium-ytterbium co-doped LaZrTa3O11 green up-conversion luminescent material and preparation method thereof
Preparation by the molten salt method of erbium ytterbium co-doped LaZrTa3O11 material, the problems of low toxicity and temperature sensitivity of NaYF4:Er3+/Yb3+ materials were solved, and upconverted phosphor with high brightness, low toxicity and high chemical stability were achieved. in a variety of application fields.
Patent Information
- Application Number
- CN202410952260.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Traditional NaYF4:Er3+/Yb3+ upconversion luminescent materials limit their application areas due to their low toxicity and low temperature sensitivity, and require a replacement material with high chemical stability and low temperature sensitivity.
The LaZrTa3O11 material is co-doped by the molten salt method, and the LaZrTa3O11 upconverter powder with a layered structure is sintered to form the LaZrTa3O11:Er3+/Yb3+ upconverter powder to ensure the high material Brightness and low toxicity.
It realizes high-efficiency energy transmission under 980nm laser excitation, presents high brightness pure green fluorescence, temperature sensitivity is 0.01221K-1, fluorescence integral intensity reaches 29.2% of NaYF4:Er3+/Yb3+, and has high chemical stability and low toxicity. Suitable for acid and alkali environment and biomedicine fields.
Smart Images

Figure CN118909630A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of up-conversion luminescent materials, and in particular to an erbium-ytterbium co-doped LaZrTa3O 11 Green up-conversion luminescent material and preparation method thereof. Background Art
[0002] Currently, NaYF4:Er 3+ / Yb 3+ Due to their outstanding fluorescence intensity, upconversion phosphors are widely used in biomedicine, solar cells, photocatalysis, non-contact temperature testing, anti-counterfeiting and plant growth.
[0003] However, fluoride has certain toxicity and low temperature sensitivity, which limits the application of NaYF4:Er 3+ / Yb 3+ Applicable fields.
[0004] Therefore, it is necessary to use oxides with high chemical stability to replace fluorides to prepare phosphors with high temperature sensitivity. Summary of the invention
[0005] The invention discloses an erbium-ytterbium co-doped LaZrTa3O 11 Green up-conversion luminescent material and preparation method thereof, under the premise of ensuring high brightness characteristics, solves the problem of traditional up-conversion luminescent material NaYF4:Er 3+ / Yb 3+ There are problems with toxicity and low temperature sensitivity.
[0006] On the one hand, the present invention provides an erbium-ytterbium co-doped LaZrTa3O 11 Green upconversion luminescent material, based on LaZrTa3O 11 is a matrix, in which Er is doped 3+ and Yb 3+ , the Er-Yb co-doped LaZrTa3O 11 The chemical formula of green upconversion luminescent material is (La a Er b Yb c )ZrTa3O 11 , where a+b+c=1.
[0007] Furthermore, in the chemical formula, a=0.94, b=0.02, c=0.04.
[0008] Erbium and ytterbium co-doped LaZrTa3O 11 Beneficial effects of green upconversion luminescent materials:
[0009] The present invention is the first to use the molten salt method to prepare LaZrTa3O with Ta2O5, La2O3, Er2O3, Yb2O3 and ZrO2 as substrates and B2O3 as solvent. 11 :Er 3+ / Yb 3+ Upconversion phosphor, LaZrTa3O 11 For the layered structure, Er 3+ / Yb 3+ The ions are distributed in a layer in a 2D distribution. The prepared phosphor has Yb 3+ Xiang Er 3+ Highly efficient energy transfer, presenting pure green fluorescence with high brightness, and temperature sensitivity of 0.01221K -1 , and the green upconversion fluorescence integral intensity reached NaYF4:Er 3+ / Yb 3+ 29.2% of the prepared LaZrTa3O 11 :Er 3+ / Yb 3+ Upconversion phosphors have the advantages of high chemical stability and low toxicity, and are expected to replace traditional NaYF4:Er in applications such as acid-base environments, high temperature environments, biomedicine, and temperature sensing. 3+ / Yb 3+ Upconversion phosphors.
[0010] Another aspect of the present invention provides an erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0011] S1: La2O3, Er2O3, Yb2O3, ZrO2, and Ta2O5 are weighed and mixed according to the molar ratio of each element in the chemical formula to obtain a mixture I;
[0012] S2: 0.7-5.5 g of the mixture I is mixed with 2-15 g of B2O3 to obtain a mixture II, and then the mixture II is sintered at 900-1200° C. for 4-24 hours;
[0013] S3: The sintered sample is filtered, dried, acid-washed, filtered again, and dried again to obtain an up-conversion luminescent material.
[0014] Furthermore, in S1, the La2O3, Er2O3, Yb2O3, ZrO2, and Ta2O5 are weighed respectively according to a molar ratio of 0.94:0.02:0.04:1:3.
[0015] Furthermore, in S3, the specific method of pickling is: using HCl with pH=0 and pickling for 6 hours.
[0016] Furthermore, the La2O3 is heat-treated at 900°C for 2 hours before being weighed and mixed; the heat treatment is performed to remove moisture from the La2O3, which helps to improve the purity and stability of the material and facilitate the subsequent successful acquisition of a single-phase phosphor material sample.
[0017] Furthermore, in S3, the drying temperature is 80°C and the drying time is 2 hours.
[0018] Furthermore, in S1, the purity of La2O3, Er2O3, Yb2O3, ZrO2, and Ta2O5 is 99.9%.
[0019] Erbium and ytterbium co-doped LaZrTa3O 11 Beneficial effects of the preparation method of green upconversion luminescent material:
[0020] The method uses La2O3, Er2O3, Yb2O3, ZrO2, and Ta2O5 as matrix raw materials, adds B2O3 for sintering, and sintering in air. B2O3, as a solvent, can dissolve the oxides at high temperature, so that the oxides form free ions and react to form crystals, and finally prepare the hexagonal LaZrTa3O 11 :Er 3 + / Yb 3 + Up-conversion phosphor, acid washing is used to remove B2O3 and other impurities on the surface of the sample, so that the surface of the sample is smoother, the prepared phosphor material has higher purity, and the fluorescence intensity can be improved; this method uses a relatively low temperature molten salt method to prepare the phosphor, which makes it easier to control the morphology and growth direction of the material particles, and the Ta2O5 used in the raw material of this method is cheaper, stable in nature, non-toxic, non-hazardous, and safer. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0022] Figure 1 The XRD test result diagram of the up-conversion luminescent materials of Example 1, Example 2 and Example 3;
[0023] Figure 2 The up-conversion fluorescence spectra of the up-conversion luminescent materials of Example 1, Example 2 and Example 3 under 980nm laser excitation;
[0024] Figure 3 The XRD test result diagram of the up-conversion luminescent materials of Example 4, Example 5 and Example 6;
[0025] Figure 4 The up-conversion fluorescence spectra of the up-conversion luminescent materials of Example 4, Example 5 and Example 6 under 980nm laser excitation;
[0026] Figure 5 The XRD test result diagram of the up-conversion luminescent materials of Example 8, Example 9, Example 10 and Example 11;
[0027] Figure 6 The up-conversion fluorescence spectra of the up-conversion luminescent materials of Example 8, Example 9, Example 10 and Example 11 under 980nm laser excitation;
[0028] Figure 7 The SEM images of the up-conversion luminescent materials of Example 4, Example 7, Example 9 and Example 10;
[0029] Figure 8 Under 980nm laser excitation, the upconversion luminescent material of Example 10 and NaYF4:Er 3+ / Yb 3+ Up-conversion fluorescence spectrum of
[0030] Fig. 9 The temperature-dependent up-conversion fluorescence spectrum of the up-conversion luminescent material of Example 10 under 980nm laser excitation;
[0031] Fig.10 is a graph showing the relationship between the fluorescence branching ratio LIR value and temperature of the up-conversion luminescent material of Example 10;
[0032] Fig.11 Graph showing the relationship between the relative temperature sensitivity of the up-conversion luminescent material of Example 10 and temperature. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example
[0035] Embodiment 1:
[0036] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0037] S1: La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 are used as matrix materials. 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0038] S2: Add 15 g B2O3 to mixture I (i.e., the mass ratio of the matrix material to the solvent B2O3 is about 1:1 (1:1.0456)) , After mixing, sintering was performed at 900 °C for 4 h in a resistance furnace;
[0039] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0040] Embodiment 2:
[0041] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0042] S1: La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 are used as matrix materials. 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0043] S2: Add 15 g of B2O3 to mixture I, and then sinter in a resistance furnace at 1100 °C for 4 h;
[0044] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0045] Embodiment 3:
[0046] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0047] S1: La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 are used as matrix materials. 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0048] S2: Add 15 g of B2O3 to mixture I, and then sinter in a resistance furnace at 1200 °C for 4 h;
[0049] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0050] Embodiment 4:
[0051] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0052] S1: La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 are used as matrix materials. 3+ :Er 3+ :Yb 3+ :Zr 4+:Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0053] S2: Add 15 g of B2O3 to mixture I, and then sinter in a resistance furnace at 1100 °C for 24 h;
[0054] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0055] Embodiment 5:
[0056] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0057] S1: La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 are used as matrix materials. 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0058] S2: Add 15 g of B2O3 to mixture I and sinter at 1150 °C in a resistance furnace for 24 h;
[0059] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0060] Embodiment 6:
[0061] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0062] S1: La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 are used as matrix materials. 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0063] S2: Add 15 g of B2O3 to mixture I, and then sinter in a resistance furnace at 1200 °C for 24 h;
[0064] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0065] Embodiment 7:
[0066] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0067] S1: La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 are used as matrix materials. 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0068] S2: Add 15 g of B2O3 to mixture I, and then sinter in a resistance furnace at 1100 °C for 24 h;
[0069] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven at 80°C for 2 hours for drying. The dried sample was placed in a pH = 0 HCl solution for acid washing for 6 hours, and then the sample was filtered again, and then placed in an oven at 80°C for drying for 2 hours to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0070] Embodiment 8:
[0071] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0072] S1: Take La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 as the matrix materials, according to La 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0073] S2: Add 2 g of B2O3 to mixture I, and then sinter in a resistance furnace at 1100 °C for 24 h;
[0074] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0075] Embodiment 9:
[0076] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0077] S1: Take La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 as the matrix materials, according to La 3+ :Er 3+ :Yb 3+ :Zr4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0078] S2: Add 3 g of B2O3 to mixture I and sinter in a resistance furnace at 1100 °C for 24 h;
[0079] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0080] Embodiment 10:
[0081] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0082] S1: Take La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 as the matrix materials, according to La 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0083] S2: Add 3 g of B2O3 to mixture I and sinter in a resistance furnace at 1100 °C for 24 h;
[0084] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven at 80°C for 2 hours for drying. The dried sample was placed in a pH = 0 HCl solution for acid washing for 6 hours, and then the sample was filtered again, and then placed in an oven at 80°C for drying for 2 hours to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O11 .
[0085] Embodiment 11:
[0086] Erbium-ytterbium co-doped LaZrTa3O 11 The method for preparing a green up-conversion luminescent material comprises the following steps:
[0087] S1: Take La2O3, Er2O3, Yb2O3, ZrO2, Ta2O5 as the matrix materials, according to La 3+ :Er 3+ :Yb 3+ :Zr 4+ :Ta 5+ =0.94:0.02:0.04:1:3 molar ratio, 0.4620g La2O3, 0.0115g Er2O3, 0.0238g Yb2O3, 0.3718g ZrO2 and 2g Ta2O5 were taken, mixed and ground in a mortar for 30 minutes to obtain mixture I, La2O3 was previously heat-treated at 900°C for 2h;
[0088] S2: Add 5 g of B2O3 to mixture I and sinter in a resistance furnace at 1100 °C for 24 h;
[0089] S3: The sintered sample was filtered, and then the obtained solid was placed in an oven and dried at 80°C for 2h to obtain an upconversion luminescent material (La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 .
[0090] The temperature, time, solvent amount, and presence or absence of an acid wash step set for Examples 1-11 are shown in Table 1 below.
[0091] Table 1: Parameters and dosage table of Examples 1-11
[0092] Sample No. temperature time Solvent amount With or without pickling Example 1 900 4 15g No pickling Example 2 1100 4 15g No pickling Example 3 1200 4 15g No pickling Example 4 1100 24 15g No pickling Example 5 1150 24 15g No pickling Example 6 1200 24 15g No pickling Example 7 1100 24 15g Pickling Example 8 1100 24 2g No pickling Example 9 1100 24 3g No pickling Example 10 1100 24 3g Pickling Embodiment 11 1100 24 5g No pickling
[0093] Comparative Example:
[0094] Existing NaYF4:Er 3+ / Yb 3+ Luminescent material (Shenzhen Zhanwanglong Technology Co., Ltd., 980nm infrared up-conversion excited green NaYF4 anti-counterfeiting phosphor identification biological probe).
[0095] Performance testing
[0096] 1. The performance of the up-conversion luminescent materials prepared in the above Examples 1-10 and Comparative Example 1 was tested using a copper target, an XRD-Rigaku D / MAX RE, and an incident wavelength of
[0097] Test results see Figure 1 , Figure 3 , Figure 5 :
[0098] 2. The up-conversion luminescent materials prepared in the above Examples 1-10 and Comparative Example 1 were excited by a 980 nm laser (18.09 W / cm 2 ) was tested for relative green light integrated intensity (green light phosphor performance). The 980nm laser was produced by Changchun New Industry Company. The laser power density ranged from 0 to 60W / cm 2 The test instrument is Hitachi F-4600 fluorescence spectrometer. The test results are shown in Figure 2 , Figure 4 , Figure 6 , Figure 8 .
[0099] Figure 1 The results show that the LaZrTa3O prepared by the molten salt method using 15 g B2O3 as solvent and sintering at 900°C (Example 1), 1100°C (Example 2) and 1200°C (Example 3) for 4 h respectively has a good thermal conductivity. 11 :0.02Er 3+ / 0.04Yb 3+ ((La 0.94 Er 0.02 Yb 0.04 )ZrTa3O 11 ) samples were compared with the results of relative fluorescence intensity. Figure 1 It can be seen that single-phase LaZrTa3O cannot be generated under 900℃ 11 :0.02Er 3+ / 0.04Yb 3+ , single-phase LaZrTa3O can be generated at 1100℃ 11 :0.02Er 3+ / 0.04Yb 3+ When the temperature rises to 1200℃, a small amount of Ta2O5 and ZrO2 impurities appear in the sample; Figure 2 It can be seen that as the reaction temperature increases from 900℃ to 1200℃, the upconversion fluorescence intensity of the sample increases accordingly; Figure 3 It can be seen that in Example 4, under the condition of a reaction time of 24 h, the sintering temperature of 1100 °C is the optimal temperature, and the prepared sample is a single-phase LaZrTa3O 11:0.02Er 3+ / 0.04Yb 3+ As the temperature increases, the sample gradually transforms into β-Ta2O5. When the temperature reaches 1200℃ (Example 6), the sample structure is consistent with β-Ta2O5. Therefore, the preparation of LaZrTa3O 11 :0.02Er 3+ / 0.04Yb 3+ The best conditions are sintering at 1100℃ for 24h; Figure 4 It can be seen that in Examples 4-6, the single-phase LaZrTa3O prepared by sintering at 1100°C for 24h in Example 4 11 :0.02Er 3+ / 0.04Yb 3+ Has the best upconversion fluorescence intensity; such as Figure 5 As shown in the figure, the XRD results of the samples prepared by using 2g, 3g, and 5g B2O3 solvent and acid washing treatment in Examples 8-11 respectively have no impurity peaks, that is, the prepared LaZrTa3O 11 :0.02Er 3+ / 0.04Yb 3+ Phosphors are all single-phase; Figure 6 As shown, the sample prepared by using 3g B2O3 solvent in Example 10 has the best up-conversion fluorescence intensity, and the fluorescence intensity can be further improved after acid washing. Figure 8 It can be seen that the fluorescence integrated intensity of the up-conversion green phosphor prepared in Example 10 reaches that of NaYF4:Er 3+ / Yb 3+ The emission light is around 500nm, with high brightness and pure green characteristics.
[0100] 3. Scanning electron microscope (SEM-ZEISS Sigma 300, Germany) was used to scan the upconversion luminescent materials prepared in Example 4, Example 7, Example 9 and Example 10. The SEM images are as follows: Figure 7 As shown, from Figure 7 It can be seen that the single-phase LaZrTa3O prepared in Example 10 11 :0.02Er 3+ / 0.04Yb 3+ The morphology of the upconversion luminescent material is a regular hexagonal plate. After acid washing, B2O3 and other small molecular impurities on the surface of the sample are removed, and its morphology becomes smoother, so the upconversion fluorescence intensity of the sample is improved.
[0101] 4. Test the upconversion luminescent material prepared in Example 10 under 980nm laser excitation (5.48W / cm2 ), in the temperature range of 303 to 723 K, LaZrTa3O 11 :0.02Er 3+ / 0.04Yb 3+ Temperature-dependent upconversion spectra, see Fig. 9 ,Depend on Fig. 9 It can be seen that Er 3+ Ionic 2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 →4I 15 / 2 and 4 F 9 / 2 → 4 I 15 / 2 The transition emission decreases with increasing temperature.
[0102] according to Fig. 9 The relationship curve between the IH and IS fluorescence intensity branching ratio (LIR value) and temperature, and the relationship curve between the LIR value and temperature T calculated from the spectral data in can be calculated by the following formula:
[0103]
[0104] I H For Er 3+ of 2 H 11 / 2 → 4 I 15 / 2 Emission fluorescence integrated intensity value;
[0105] I S For Er 3+ of 4 S 3 / 2 → 4 I 15 / 2 The value of the integrated intensity of emitted fluorescence; B is a constant, k B is the Boltzmann constant, ΔE is 2 H 11 / 2 and 4 S 3 / 2 The band gap between energy levels.
[0106] The fitted function is LIR = 33.80exp(-1119.44 / T), see Fig.10 ,from Fig.10 It can be seen that the LIR value (I H / I S The value) increases with the increase of temperature.
[0107] 5. Calculate the absolute temperature sensitivity S of the up-conversion luminescent material obtained in Example 10 aboveR Relationship with temperature, S R The relationship curve between temperature T can be calculated by the following formula:
[0108]
[0109] The calculation results are as follows Fig.11 As shown by Fig.11 It can be seen that the LaZrTa3O prepared in Example 10 11 :0.02Er 3+ / 0.04Yb 3+ , at 303K, the maximum relative temperature sensitivity S A 0.01221K -1 , proving that LaZrTa3O 11 :0.02Er 3+ / 0.04Yb 3+ Luminescent materials have certain application prospects in the field of photothermal sensing.
[0110] Therefore, the present invention prepares LaZrTa3O 11 :0.02Er 3+ / 0.04Yb 3+ The optimal sintering condition of the luminescent material is sintering at 1100℃ for 24h. After acid washing, the LaZrTa3O in the prepared upconversion luminescent material can be 11 The LaZrTa3O prepared by the present invention is single-phase and has a smoother morphology. 11 :0.02Er 3+ / 0.04Yb 3+ Upconversion luminescent materials have the characteristics of pure green high brightness, high chemical stability and low toxicity, and are expected to replace commercial NaYF4:Er in some special application fields. 3+ / Yb 3+ Phosphor.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. Erbium-ytterbium co-doped LaZrTa3O 11 A green up-conversion luminescent material, characterized in that LaZrTa3O 11 is a matrix, in which Er is doped 3+ and Yb 3+ , the Er-Yb co-doped LaZrTa3O 11 The chemical formula of green upconversion luminescent material is (La a Er b Yb c )ZrTa3O 11 , where a+b+c=1.
2. The Er-Yb co-doped LaZrTa3O according to claim 1 11 A green up-conversion luminescent material, characterized in that In the chemical formula, a=0.94, b=0.02, c=0.
04.
3. An Er-Yb co-doped LaZrTa3O as claimed in any one of claims 1 to 2 11 The method for preparing a green up-conversion luminescent material is characterized in that: The following steps are involved: S1: La2O3, Er2O3, Yb2O3, ZrO2, and Ta2O5 are weighed and mixed according to the molar ratio of each element in the chemical formula to obtain a mixture I; S2: 0.7-5.5 g of the mixture I is mixed with 2-15 g of B2O3 to obtain a mixture II, and then the mixture II is sintered at 900-1200° C. for 4-24 hours; S3: The sintered sample is filtered, dried, acid-washed, filtered again, and dried again to obtain an up-conversion luminescent material.
4. Erbium-ytterbium co-doped LaZrTa3O according to claim 3 11 The method for preparing a green up-conversion luminescent material is characterized in that: In S1, the La2O3, Er2O3, Yb2O3, ZrO2, and Ta2O5 are weighed respectively according to the molar ratio of 0.94:0.02:0.04:1:
3.
5. Erbium-ytterbium co-doped LaZrTa3O according to claim 3 11 The method for preparing a green up-conversion luminescent material is characterized in that: In S3, the specific method of pickling is: using HCl with pH=0 and pickling for 6 hours.
6. Erbium-ytterbium co-doped LaZrTa3O according to claim 3 11 The method for preparing a green up-conversion luminescent material is characterized in that: The La2O3 is heat treated at 900°C for 2 hours before being weighed and mixed.
7. Erbium-ytterbium co-doped LaZrTa3O according to claim 3 11 The method for preparing a green up-conversion luminescent material is characterized in that: In S3, the drying temperature is 80°C and the drying time is 2 hours.
8. Erbium-ytterbium co-doped LaZrTa3O according to claim 3 11 The method for preparing a green up-conversion luminescent material is characterized in that: In S1, the purity of La2O3, Er2O3, Yb2O3, ZrO2 and Ta2O5 is 99.9%.
Citation Information
Patent Citations
Single-matrix luminescent material for white-light LED ss well as preparation method and application thereof
CN112745848A
Method for preparing erbium-ytterbium-doped LaTa7O19 up-conversion fluorescent powder through molten salt method and application