Method for preparing high-performance coal water slurry from solid waste coupled wastewater
Through solid waste grading pretreatment and step-by-step pulping method, combined with the use of additives, the problem of coordinated treatment of solid waste and wastewater in coal chemical industry is solved, and high-performance water-coal slurry is prepared, which solves the resource utilization of solid waste and wastewater and The high cost problem has been dealt with, and the goal of efficient resource utilization and energy conservation and carbon reduction has been achieved.
Patent Information
- Application Number
- CN202410967775.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The solid waste and wastewater treatment of coal chemical enterprises has the risk of secondary pollution and high treatment costs, and the existing technology is difficult to achieve the full resource utilization of waste, especially the lack of effective methods for the coordinated treatment of coal chemical solid waste and wastewater.
Through solid waste grading pretreatment and step-by-step pulping method, combining the physical and chemical properties of solid waste and wastewater of different particle sizes, the mixing and grinding mechanism is used to prepare high-performance water and coal slurry, and the solid waste fine slurry and solid waste are used to use additives I and II for stirring and grinding mechanisms. Mixing of water and coal slurry is used to improve the stacking efficiency and concentration of water and coal slurry.
The preparation of high-performance coal slurry is achieved, with high concentration, good dispersion and fluidity, high stability, meeting gasification process requirements, reducing wastewater treatment costs, improving the added value of solid waste application and resource utilization efficiency .
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste and wastewater treatment and coal-water slurry preparation, and specifically relates to a method for preparing high-performance coal-water slurry by coupling solid waste with wastewater. Background Art
[0002] Coal chemical industry refers to the process of converting coal into gas, liquid and solid fuels and chemicals through thermal and catalytic processing. Coal gasification plays an important role in coal chemical industry. It is used to produce various gas fuels and is a clean energy source. The synthesis gas produced by coal gasification is the raw material for synthesizing liquid fuels, chemical raw materials and other products.
[0003] During the coal gasification process, various wastes are generated, among which the largest output is gasification ash, about tens of millions of tons per year. With the establishment of coal chemical enterprises, the output of solid waste has increased year by year in recent years. Commonly used solid waste treatment methods include incineration, landfill, composting, anaerobic digestion, etc. These methods are prone to secondary pollution and have a narrow scope of application. If solid waste is not properly managed, it will cause great harm to the atmosphere, water, soil and even the health of citizens. For coal chemical enterprises, the transportation and treatment costs of solid waste are a considerable expense.
[0004] The high-concentration wastewater generated during the coal gasification process contains heterocyclic compounds, polycyclic aromatic hydrocarbons, phenols, sulfides, cyanides and tar, etc. Its water quality components are complex, the pollutant concentration is high, the toxicity is high and the biodegradability is poor. The quality of wastewater varies due to the different types, components, gasification processes and operation methods of raw coal. The water quality characteristics of coal chemical wastewater make it difficult for conventional treatment technologies to achieve excellent treatment effects. It is necessary to use a combination of professional and targeted treatment processes, which increases the treatment cost and system operation pressure, resulting in high wastewater treatment costs, general treatment effects and unstable operations.
[0005] How to properly solve the problem of coal chemical solid waste and wastewater has always been the focus of attention from all walks of life. Considering my country's energy consumption structure dominated by coal, using water-coal slurry technology to treat coal chemical solid waste and wastewater is a practical and effective idea. In recent years, reports on the preparation of water-coal slurry using solid waste or wastewater alone are common (for example, the hydrophilic solid waste treatment and resource utilization method disclosed in CN113667520A only pulps solid waste, and requires the use of organic solvents and surfactants to modify the solid waste), but there is little research on the preparation of high-performance water-coal slurry by coupling wastewater after pretreatment of solid waste. CN113736528A discloses a method for preparing water-coal slurry and water-coal gas and its application, wherein coal gasification black water is mixed with a flocculant and then allowed to settle to obtain gray water and fine residue; sludge water is mixed with a flocculant and then allowed to settle to obtain concentrated sludge water and dilute sludge water; and granular coal, dilute sludge water, organic wastewater, water-coal slurry additives, gray water and fine residue are ground to obtain water-coal slurry. This method realizes the effective utilization of solid waste and wastewater, but does not treat and utilize concentrated sludge water, that is, does not realize the complete utilization of waste resources. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing high-performance water-coal slurry by coupling solid waste with wastewater. This method uses solid waste to replace part of the raw coal, and uses wastewater to replace slurrying water. This method can not only make full use of solid waste and wastewater to realize the resource utilization of waste, but also help achieve the company's energy conservation and carbon reduction goals.
[0007] The high-performance water-coal slurry provided by the present invention is made of the following raw materials in percentage by mass: 10% to 35% of solid waste, 28% to 58% of coal powder, 30% to 40% of waste water, and 0.05% to 0.45% of additives; the additives are composed of additive I and additive II, and the mass ratio of the additives is 1:2 to 8.
[0008] Furthermore, the high-performance water-coal slurry provided by the present invention is preferably made of the following raw materials in percentage by mass: 20% to 30% solid waste, 35% to 49% coal powder, 30% to 40% waste water, and 0.2% to 0.4% additives.
[0009] The above-mentioned solid waste is a mixture of any one or more of carbon-containing solid wastes such as gasification ash, waste activated carbon, and medicinal residues in any proportion.
[0010] The above-mentioned coal powder is low-grade coal from Shaanxi or Inner Mongolia.
[0011] The above wastewater is a mixture of any one or more of conversion condensate, fine residue filter filtrate, methanol wash liquid, and organic wastewater generated in the coal gasification process in any proportion.
[0012] The additive I is selected from a mixture of any one or more of polyacrylamide, carboxymethyl cellulose, polyacrylic acid salt and kaolin in any proportion.
[0013] The additive II is selected from any one or more of lignin sulfonate, naphthalene sulfonate formaldehyde condensate, sulfomethyl humate, benzene sulfonate, polyphosphate and a mixture thereof in any proportion.
[0014] The preparation method of the high-performance coal water slurry of the present invention comprises the following steps:
[0015] Step 1: Solid waste classification and treatment
[0016] The solid waste is crushed to less than 3 mm, heated to constant weight at 105-110°C, and the solid waste is screened by screening equipment into two particle sizes of 0.5-3 mm and less than 0.5 mm, which are called coarse solid waste and fine solid waste respectively;
[0017] Step 2: Preparation of solid waste slurry
[0018] The fine solid waste, part of the wastewater and the additive I are mixed and stirred evenly to prepare a solid waste fine slurry;
[0019] Step 3: Preparation of solid wastewater coal slurry
[0020] The coarse solid waste, coal powder, remaining wastewater and additive II are mixed and then put into a ball mill or a rod mill for grinding to obtain a solid wastewater-coal slurry;
[0021] Step 4: Preparation of high performance coal water slurry
[0022] The solid waste fine slurry and the solid waste water-coal slurry are mixed and stirred evenly to obtain a high-performance water-coal slurry.
[0023] In the above step 1, the stirring time is 10 to 30 minutes, and the stirring speed is 800 to 2000 rpm.
[0024] The mass ratio of the wastewater used in preparing the solid waste fine slurry in step 2 and preparing the solid waste water-coal slurry in step 3 is 1:3-8.
[0025] In the above step 4, the stirring time is 5 to 30 minutes, and the stirring speed is 800 to 2000 rpm.
[0026] The beneficial effects of the present invention are as follows:
[0027] 1. The solid waste in the present invention is all carbon-containing solid waste, which is graded and pre-treated, and the physicochemical properties of solid wastes with different particle sizes are used for step-by-step pulping. The finer solid waste particles can be dispersed and suspended in the wastewater system under the action of additive I to obtain solid waste fine slurry, and metal ions such as calcium and magnesium in the wastewater also have a good dispersing and stabilizing effect on fine solid waste particles. The coarser solid waste and coal powder enter the mill with the remaining wastewater under the action of additive II to obtain solid waste water-coal slurry, and various technical indicators meet the requirements of the gasification process. Finally, the solid waste fine slurry and the solid waste water-coal slurry are evenly stirred to obtain a high-performance water-coal slurry. This is because after the solid waste fine slurry is mixed with the solid waste water-coal slurry, the fine slurry of the finer particles is effectively filled between the coarser particles of the solid waste water-coal slurry, which improves the stacking efficiency of the water-coal slurry, thereby increasing the concentration of the water-coal slurry. The present invention can process a large amount of solid waste, and at the same time, wastewater is used to completely replace the traditional pulping water, and a water-coal slurry with high concentration, good dispersibility and fluidity and high stability can be prepared with a small amount of additives.
[0028] 2. The present invention combines graded pretreatment with step-by-step pulping, combines the physicochemical properties of solid wastes of different particle sizes with the quality of wastewater, and utilizes the dispersion characteristics of solid wastes of different particle sizes in wastewater for step-by-step pulping. The solid waste fine pulp adopts a mixing and stirring method, and the solid waste water-coal slurry adopts a mill pulping method. Finally, a mixing and stirring method is used to prepare a high-performance water-coal slurry. This method effectively avoids the shortcomings of insufficient material reaction and low slurry concentration in the traditional one-step mill pulping method. The prepared water-coal slurry has a high concentration, and the performance of the water-coal slurry does not change due to changes in the quality of wastewater. Various technical indicators meet the requirements of the gasification process.
[0029] 3. The present invention uses low-rank coal blended with carbonaceous solid waste in northern Shaanxi and Inner Mongolia as the research object, and couples coal chemical wastewater to prepare water-coal slurry, which not only increases the added value of solid waste, but also reduces the cost of wastewater treatment, and has a positive guiding role in water conservation and resource utilization in the coal chemical system. The present invention provides a theoretical basis for the management of waste and plays a positive role in promoting the resource utilization of waste. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with the embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0031] Example 1
[0032] The high-performance water-coal slurry of this embodiment is made of the following raw materials in percentage by mass: 20% of waste activated carbon, 44% of coal powder, 35.7% of waste water, and 0.3% of additives; the waste water is a mixture of conversion condensate, fine slag filter filtrate, and washing methanol liquid in a mass ratio of 3:6:1, and the additive is composed of polyacrylamide and sodium lignin sulfonate, and the mass ratio of polyacrylamide to sodium lignin sulfonate is 1:3.75.
[0033] The preparation method of the high-performance coal water slurry of this embodiment comprises the following steps:
[0034] Step 1: Solid waste classification and treatment
[0035] The waste activated carbon is crushed to less than 3 mm, heated to constant weight at 105°C, and screened using screening equipment to separate the waste activated carbon into two particle sizes: 0.5-3 mm and less than 0.5 mm, which are called coarse activated carbon and fine activated carbon, respectively.
[0036] Step 2: Preparation of solid waste slurry
[0037] The fine activated carbon, part of the wastewater and polyacrylamide were mixed and stirred at 1700 rpm for 10 min to obtain a solid waste fine slurry.
[0038] Step 3: Preparation of solid wastewater coal slurry
[0039] The crude activated carbon, coal powder, remaining wastewater and sodium lignin sulfonate are mixed and then put into a ball mill for grinding to obtain solid waste water coal slurry. The mass ratio of wastewater used for preparing solid waste fine slurry to that used for preparing solid waste water coal slurry is 1:5.
[0040] Step 4: Preparation of high performance coal water slurry
[0041] The solid waste fine slurry and the solid waste water-coal slurry were mixed and stirred at 1700 rpm for 12 minutes to obtain a high-performance water-coal slurry.
[0042] Example 2
[0043] The high-performance water-coal slurry of this embodiment is made of the following raw materials in percentage by mass: 20% gasification ash, 44% coal powder, 35.8% waste water, and 0.2% additives; the waste water is a mixture of conversion condensate, fine slag filter filtrate, and washing methanol liquid in a mass ratio of 2:8:1, and the additive is composed of polyacrylamide and sodium sulfomethyl humate, and the mass ratio of polyacrylamide to sodium sulfomethyl humate is 1:3.3.
[0044] The preparation method of the high-performance coal water slurry of this embodiment comprises the following steps:
[0045] Step 1: Solid waste classification and treatment
[0046] The gasification ash is crushed to less than 3 mm, heated to constant weight at 105°C, and screened using screening equipment to separate the gasification ash into two particle sizes: 0.5-3 mm and less than 0.5 mm, which are called coarse ash and fine ash, respectively.
[0047] Step 2: Preparation of solid waste slurry
[0048] The fine ash, part of the wastewater and polyacrylamide were mixed and stirred at 1500 rpm for 15 minutes to obtain a solid waste fine slurry.
[0049] Step 3: Preparation of solid wastewater coal slurry
[0050] The coarse ash, coal powder, remaining wastewater and sodium sulfomethyl humate are mixed and then put into a ball mill for grinding to obtain solid waste water coal slurry. The mass ratio of the wastewater used to prepare the solid waste fine slurry and the wastewater used to prepare the solid waste water coal slurry is 1:5.
[0051] Step 4: Preparation of high performance coal water slurry
[0052] The solid waste fine slurry and the solid waste water-coal slurry were mixed and stirred at 1500 rpm for 15 minutes to obtain a high-performance water-coal slurry.
[0053] Example 3
[0054] The high-performance water-coal slurry of this embodiment is made of the following raw materials in percentage by mass: 15% medicinal residue, 49% coal powder, 35.8% waste water, and 0.2% additives; the waste water is a mixture of conversion condensate, fine residue filter filtrate, and washing methanol liquid in a mass ratio of 2:8:1, and the additive is composed of carboxymethyl cellulose and sodium benzenesulfonate, and the mass ratio of carboxymethyl cellulose to sodium benzenesulfonate is 1:5.7.
[0055] The preparation method of the high-performance coal water slurry of this embodiment comprises the following steps:
[0056] Step 1: Solid waste classification and treatment
[0057] The drug residue is crushed to less than 3 mm, heated to constant weight at 105°C, and screened using screening equipment to separate the drug residue into two particle size grades: 0.5-3 mm and less than 0.5 mm, which are called coarse drug residue and fine drug residue respectively.
[0058] Step 2: Preparation of solid waste slurry
[0059] The fine drug residue, part of the waste water and carboxymethyl cellulose were mixed and stirred at 1300 rpm for 20 min to obtain a solid waste fine slurry.
[0060] Step 3: Preparation of solid wastewater coal slurry
[0061] The crude drug residue, coal powder, remaining wastewater and sodium benzenesulfonate are mixed and then put into a rod mill for grinding to obtain solid waste water-coal slurry. The mass ratio of wastewater used to prepare solid waste fine slurry and solid waste water-coal slurry is 1:6.
[0062] Step 4: Preparation of high performance coal water slurry
[0063] The solid waste fine slurry and the solid waste water-coal slurry were mixed and stirred at 1300 rpm for 22 minutes to obtain a high-performance water-coal slurry.
[0064] Example 4
[0065] The high-performance water-coal slurry of this embodiment is made of the following raw materials in percentage by mass: 12.5% gasification ash, 12.5% waste activated carbon, 41% coal powder, 35.65% waste water, and 0.35% additives; the waste water is a mixture of conversion condensate and washing methanol liquid in a mass ratio of 3:1, and the additive is composed of sodium polyacrylate and sodium naphthalenesulfonate formaldehyde condensate, and the mass ratio of sodium polyacrylate and sodium naphthalenesulfonate formaldehyde condensate is 1:6.25.
[0066] The preparation method of the high-performance coal water slurry of this embodiment comprises the following steps:
[0067] Step 1: Solid waste classification and treatment
[0068] The gasification ash and waste activated carbon are mixed in a mass ratio of 1:1 as mixed solid waste, first crushed to less than 3 mm, heated to constant weight at 105°C, and screened using screening equipment to separate the mixed solid waste into two particle size grades: 0.5-3 mm and less than 0.5 mm, which are called coarse solid waste and fine solid waste, respectively.
[0069] Step 2: Preparation of solid waste slurry
[0070] The fine solid waste, part of the wastewater and sodium polyacrylate were mixed and stirred at 1200 rpm for 25 minutes to obtain a solid waste fine slurry.
[0071] Step 3: Preparation of solid wastewater coal slurry
[0072] The coarse solid waste, coal powder, residual wastewater and sodium naphthalenesulfonate formaldehyde condensate are mixed and then put into a rod mill for grinding to obtain solid waste water-coal slurry. The mass ratio of wastewater used to prepare solid waste fine slurry and solid waste water-coal slurry is 1:4.5.
[0073] Step 4: Preparation of high performance coal water slurry
[0074] The solid waste fine slurry and the solid waste water-coal slurry were mixed and stirred at 1200 rpm for 25 minutes to obtain a high-performance water-coal slurry.
[0075] Example 5
[0076] The high-performance water-coal slurry of this embodiment is made of the following raw materials in percentage by mass: 10% gasification ash, 10% waste activated carbon, 10% medicinal residue, 33% coal powder, 36.6% waste water, and 0.4% additives; the waste water is a mixture of conversion condensate and fine residue filter filtrate in a mass ratio of 2:1, and the additive is composed of carboxymethyl cellulose and sodium naphthalenesulfonate formaldehyde condensate, and the mass ratio of carboxymethyl cellulose to sodium naphthalenesulfonate formaldehyde condensate is 1:7.2.
[0077] The preparation method of the high-performance coal water slurry of this embodiment comprises the following steps:
[0078] Step 1: Solid waste classification and treatment
[0079] Gasification ash, waste activated carbon and medicinal residue are mixed in a mass ratio of 1:1:1 as mixed solid waste, first crushed to less than 3 mm, heated to constant weight at 105°C, and screened using screening equipment to separate the mixed solid waste into two particle size grades: 0.5-3 mm and less than 0.5 mm, which are called coarse solid waste and fine solid waste, respectively.
[0080] Step 2: Preparation of solid waste slurry
[0081] The fine solid waste, part of the wastewater and carboxymethyl cellulose were mixed and stirred at 1300 rpm for 25 minutes to obtain a solid waste fine slurry.
[0082] Step 3: Preparation of solid wastewater coal slurry
[0083] The coarse solid waste, coal powder, residual wastewater and sodium naphthalenesulfonate formaldehyde condensate are mixed and then put into a rod mill for grinding to obtain solid waste water-coal slurry. The mass ratio of the wastewater used to prepare the solid waste fine slurry and the wastewater used to prepare the solid waste water-coal slurry is 1:4.
[0084] Step 4: Preparation of high performance coal water slurry
[0085] The solid waste fine slurry and the solid waste water-coal slurry were mixed and stirred at 1300 rpm for 25 minutes to obtain a high-performance water-coal slurry.
[0086] Comparative Example 1
[0087] The water-coal slurry in this comparative example is made of the following raw materials in percentage by mass: 12.5% of gasification ash, 12.5% of waste activated carbon, 41% of coal powder, 35.65% of waste water, and 0.35% of additives; the waste water is a mixture of conversion condensate and washing methanol liquid in a mass ratio of 3:1, and the additive is composed of sodium polyacrylate and sodium naphthalenesulfonate formaldehyde condensate, and the mass ratio of sodium polyacrylate and sodium naphthalenesulfonate formaldehyde condensate is 1:6.25.
[0088] The preparation method of the water-coal slurry in this comparative example is: gasification ash and waste activated carbon are mixed in a mass ratio of 1:1 as mixed solid waste, and then the mixed solid waste, coal powder, waste water, sodium polyacrylate and sodium naphthalenesulfonate formaldehyde condensate are mixed and ground in a rod mill to obtain water-coal slurry.
[0089] Comparative Example 2
[0090] The water-coal slurry in this comparative example is made of the following raw materials in percentage by mass: 12.5% of gasification ash, 12.5% of waste activated carbon, 41% of coal powder, 35.65% of waste water, and 0.35% of additives; the waste water is a mixture of conversion condensate and washing methanol liquid in a mass ratio of 3:1, and the additive is composed of sodium polyacrylate and sodium naphthalenesulfonate formaldehyde condensate, and the mass ratio of sodium polyacrylate and sodium naphthalenesulfonate formaldehyde condensate is 1:6.25.
[0091] The preparation method of the water-coal slurry of this comparative example comprises the following steps:
[0092] Step 1: Prepare solid waste slurry
[0093] The gasification ash and waste activated carbon were mixed in a mass ratio of 1:1 as mixed solid waste, mixed with part of the wastewater and sodium polyacrylate, and stirred at 1200 rpm for 25 minutes to obtain a solid waste slurry.
[0094] Step 2: Prepare coal water slurry
[0095] The solid waste slurry, coal powder, remaining wastewater and sodium naphthalenesulfonate formaldehyde condensate are mixed and then put into a rod mill for grinding to obtain water-coal slurry. The mass ratio of the solid waste slurry to the wastewater used for preparing the water-coal slurry is 1:2.
[0096] The technical indicators of the water-coal slurries prepared in the above Examples 1 to 5 and Comparative Examples 1 to 2 were tested, and the experimental results are shown in
[0097] Table 1. Table 1 Coal-water slurry test data
[0098] Serial number concentration / % Viscosity / mPa.s pH Liquidity Stability 24h water separation rate / % Example 1 63.3 760.1 8.2 Continuous Flow 2.8 Example 2 63.9 813.3 8.2 Continuous Flow 2.7 Example 3 63.8 881.5 8.3 Continuous Flow 2.9 Example 4 65.6 996.7 8.1 Continuous Flow 2.9 Example 5 63.9 965.2 8.3 Continuous Flow 3.0 Comparative Example 1 61.7 1102.0 8.4 Intermittent flow 6.2 Comparative Example 2 62.4 1010.8 8.2 Intermittent flow 6.7
[0099] As shown in Table 1, the coal water slurry prepared in Examples 1 to 5 of the present invention has a concentration of 63% to 66% and a viscosity of <1000 mPa.s, and has good flowability and stability, continuous flow, and a 24h water separation rate of ≤3%. In the comparative example, the solid waste was not graded and pre-treated, and the performance indicators of the coal water slurry were reduced regardless of whether the pulping was performed using a one-step mill or a two-step mill. The coal water slurry had a lower concentration, a viscosity of >1000 mPa.s, poor flowability, and a higher water separation rate.
Claims
1. A method for preparing high-performance coal-water slurry by coupling solid waste with wastewater, characterized in that The high-performance coal-water slurry is made of the following raw materials in percentage by mass: 10% to 35% of solid waste, 28% to 58% of coal powder, 30% to 40% of waste water, and 0.05% to 0.45% of additives; the additives are composed of additive I and additive II, and the mass ratio of the two is 1:2 to 8; The preparation method of the high-performance coal water slurry comprises the following steps: Step 1: Solid waste classification and treatment The solid waste is crushed to less than 3 mm, heated to constant weight at 105-110°C, and the solid waste is screened by screening equipment into two particle sizes of 0.5-3 mm and less than 0.5 mm, which are called coarse solid waste and fine solid waste respectively; Step 2: Preparation of solid waste slurry The fine solid waste, part of the wastewater and additive I are mixed and stirred evenly to obtain a solid waste fine slurry; the additive I is selected from a mixture of any one or more of polyacrylamide, carboxymethyl cellulose, polyacrylic acid salt and kaolin; Step 3: Preparation of solid wastewater coal slurry The crude solid waste, coal powder, residual wastewater and additive II are mixed and then put into a ball mill or a rod mill for grinding to obtain a solid wastewater coal slurry; the additive II is selected from any one or more mixtures of lignin sulfonate, naphthalene sulfonate formaldehyde condensate, sulfomethyl humate, benzene sulfonate, polyphosphate; Step 4: Preparation of high performance coal water slurry The solid waste fine slurry and the solid waste water-coal slurry are mixed and stirred evenly to obtain a high-performance water-coal slurry; The mass ratio of wastewater used in the preparation of solid waste fine slurry and solid waste water-coal slurry is 1:3-8.
2. The method for preparing high-performance coal water slurry from solid waste coupled wastewater according to claim 1, characterized in that The high performance coal water slurry is made of the following raw materials in percentage by weight: Solid waste 20%~30%, coal powder 35%~49%, wastewater 30%~40%, additives 0.2%~0.4%.
3. The method for preparing high-performance coal water slurry from solid waste coupled wastewater according to claim 1 or 2, characterized in that: The solid waste is a mixture of any one or more of gasification ash, waste activated carbon and medicinal residue.
4. The method for preparing high-performance coal water slurry from solid waste coupled wastewater according to claim 1 or 2, characterized in that: The coal powder is low-rank coal from Shaanxi or Inner Mongolia.
5. The method for preparing high-performance coal water slurry from solid waste coupled wastewater according to claim 1 or 2, characterized in that: The wastewater is a mixture of any one or more of conversion condensate, fine residue filter filtrate, methanol wash liquid, and organic wastewater generated in a coal gasification process.
6. The method for preparing high-performance coal water slurry from solid waste coupled wastewater according to claim 1, characterized in that: In step 1, the stirring time is 10 to 30 minutes, and the stirring speed is 800 to 2000 rpm.
7. The method for preparing high-performance coal water slurry from solid waste coupled wastewater according to claim 1, characterized in that: In step 4, the stirring time is 5 to 30 minutes, and the stirring speed is 800 to 2000 rpm.
Citation Information
Patent Citations
Hydrophilic solid waste treatment and resource utilization method
CN113667520A
Preparation method of coal water slurry and water gas and application thereof
CN113736528A