Method for realizing selective leaching of copper and enrichment of precious metals by microwave treatment of carbonylation tailings
Through grinding-microwave pretreatment-sulfuric acid leaching-pressurized reduction leaching technology, the carbonylated tail material is treated using microwave technology, and the separation of copper and nickel and the enrichment of precious metals is achieved, and resource utilization and environmental protection in the existing technology are solved. The problem of simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202410988760.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Carbonated tailings contain a large amount of copper and precious metals, but the existing technology cannot effectively utilize resources and protect the environment. New technologies need to be developed to achieve selective copper leaching and precious metal enrichment.
The grinding-microwave pretreatment-sulfuric acid leaching-pressurized reduction leaching process is adopted to achieve the separation of copper and nickel by microwave treatment, and the precious metals are enriched through pressurized reduction.
Selective leaching of copper and enrichment of precious metals are achieved, the process is simplified, the cost is reduced, and the precious metal enrichment slag can be directly connected to the existing precious metal production process.
Smart Images

Figure BDA0004958270610000041 
Figure BDA0004958270610000051 
Figure BDA0004958270610000052
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nickel-cobalt smelting, and in particular discloses a method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings. Background Art
[0002] The main raw material for the production of carbonyl nickel is the water-quenched alloy obtained by quenching the primary alloy produced by high-matte grinding and flotation of nickel smelters. Under the carbonylation reaction conditions, nickel and iron in the water-quenched alloy generate gaseous carbonyls that are separated, and the solid residue after carbonylation extraction of nickel and iron is the carbonylation tailings. During carbonylation, the precious metals in the water-quenched alloy do not undergo carbonylation reaction, and are almost all enriched in the carbonylation tailings. In addition, the copper brought by the original high-matte nickel is enriched in the carbonylation tailings along with the water-quenched alloy. At the same time, during the high-matte nickel grinding and magnetic separation process, some sulfide phases of nickel, copper and other materials will also enter the carbonylation tailings along with the water-quenched alloy. Therefore, the carbonylation tailings contain a large amount of copper, nickel and precious metals. At present, the carbonylation tailings are stored after nitrogen disinfection and replacement and high-temperature detoxification in a reduction furnace, which is not conducive to comprehensive resource utilization and environmental protection. New technologies need to be developed to adapt to new materials. Summary of the invention
[0003] The invention proposes a method for selectively leaching copper and enriching precious metals by microwave treating carbonylation tailings, which has a simple process and low cost, can realize opening of nickel, copper and precious metals respectively, and utilizes microwave technology to improve the leaching rate of copper in carbonylation tailings.
[0004] To achieve the above object, the method of microwave treatment of carbonylation tailings to achieve copper selective leaching and precious metal enrichment is characterized in that it comprises the following steps:
[0005] a) Grinding: The carbonylation tailings are ground and the particle size is controlled at -150 to -200 mesh;
[0006] b) microwave treatment: adding the carbonylation tailings obtained in step a) into a microwave rotary kiln for microwave pretreatment;
[0007] c) Sulfuric acid leaching: subjecting the microwave-treated carbonylation tailings obtained in step b) to leaching with sulfuric acid at normal pressure, and after the reaction is completed, solid-liquid separation is performed to obtain copper sulfate leaching solution and nickel-containing precious metal leaching residue;
[0008] d) pressure reduction leaching: the nickel-containing precious metal leaching residue obtained in step c) is subjected to pressure reduction leaching, and after the reaction is completed, the solid-liquid separation is performed to obtain the nickel-containing leaching solution and the precious metal-enriched residue.
[0009] In the technical solution of the method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings of the present invention, the further preferred technical solution features are:
[0010] 1. The carbonyl tailings are obtained by carbonylating an alloy obtained by a magnetic separation process to produce carbonyl nickel from a high-grade nickel matte obtained by pyrometallurgical iron blowing of nickel-copper sulfide ore;
[0011] 2. In the step b), the microwave pretreatment is performed with a power of 6 kW to 10 kW and a microwave time of 90 to 540 s;
[0012] 3. In the step b), the microwave pretreatment is performed with a control power of 8 kW and a microwave time of 320 s;
[0013] 4. In the step c), the concentration of sulfuric acid in the atmospheric leaching is 60-200 g / L, the leaching temperature is 70-95° C., the leaching time is 4-6 h, and the leaching liquid-to-solid ratio is 9-15:1;
[0014] 5. In the step c), the concentration of sulfuric acid in the atmospheric leaching is 180 g / L, the leaching temperature is 85° C., the leaching time is 5 h, and the leaching liquid-to-solid ratio is 12:1;
[0015] 6. In the step d), the amount of sulfuric acid used for pressurized reduction leaching is 0.8 to 1.2 times the theoretical amount of nickel leached, the leaching temperature is 130 to 150°C, the leaching time is 2 to 6 hours, the leaching liquid-solid ratio is 6 to 10:1, and the sulfur dioxide partial pressure is 0.1 to 0.3 MPa;
[0016] 7. In the step d), the amount of sulfuric acid used for pressurized reduction leaching is 1 times the theoretical amount of nickel to be leached, the leaching temperature is 140° C., the leaching time is 4 h, the leaching liquid-to-solid ratio is 8:1, and the sulfur dioxide partial pressure is 0.2 MPa.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The present invention aims at the solid residue carbonyl tailings after the carbonylation extraction of nickel and iron in the production of nickel carbonyl, and proposes a method for selectively leaching copper and enriching precious metals by microwave treatment of carbonyl tailings. The method utilizes a grinding-microwave pretreatment-sulfuric acid leaching-pressure reduction leaching process to achieve the separation of valuable metals such as copper and nickel and the enrichment of precious metals.
[0019] 2. The method of the present invention realizes the separation of nickel and copper through microwave pretreatment-normal pressure leaching, shortens the process and reduces the cost.
[0020] 3. The method of the present invention separates nickel from precious metals through pressurized reduction leaching to achieve the effect of precious metal enrichment. The obtained precious metal enriched slag can be directly connected to the existing precious metal production process. DETAILED DESCRIPTION
[0021] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Example 1, a method for achieving copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings, comprising the following steps:
[0023] a) Grinding: The carbonylation tailings are ground and the particle size is controlled at -150 to -200 mesh;
[0024] b) microwave treatment: adding the carbonylation tailings obtained in step a) into a microwave rotary kiln for microwave pretreatment;
[0025] c) Sulfuric acid leaching: subjecting the microwave-treated carbonylation tailings obtained in step b) to leaching with sulfuric acid at normal pressure, and after the reaction is completed, solid-liquid separation is performed to obtain copper sulfate leaching solution and nickel-containing precious metal leaching residue;
[0026] d) Pressure reduction leaching: The nickel-containing precious metal leaching residue obtained in step c) is subjected to pressure reduction leaching, and after the reaction is completed, the solid-liquid separation is performed to obtain a nickel-containing leaching solution and a precious metal enriched residue. The process of the present invention is simple, and a method for selectively leaching copper by low-cost microwave treatment of carbonylation tailings is realized, and nickel, copper and precious metals are opened separately. The microwave technology is used to increase the leaching rate of copper in the carbonylation tailings, and nickel and copper are separated, and nickel and precious metals are separated, so as to finally achieve the purpose of enriching precious metals.
[0027] Example 2. According to the method for achieving selective leaching of copper and enrichment of precious metals by microwave treatment of carbonylation tailings as described in Example 1, the carbonylation tailings are obtained by carbonylating an alloy obtained by a magnetic separation process to produce carbonyl nickel after high nickel matte is obtained by pyrometallurgical blowing of nickel sulfide copper ore, and the main components are expressed in weight percentage as follows: Ni: 6-10%, Cu: 65-75%, Fe: 0.8-5%, S: 10-15%, Ag: 300-500g / t, ∑Au+Pd+Pt: 800-1500g / t.
[0028] Example 3, in the method for selective leaching of copper and enrichment of precious metals by microwave treatment of carbonylation tailings according to Example 1 or 2, the microwave pretreatment in step b) is controlled to have a power of 6 kW to 10 kW and a microwave time of 90 to 540 s.
[0029] Example 4, in the method for achieving copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to any one of Examples 1-3, the microwave pretreatment in step b) is controlled with a power of 8 kW and a microwave time of 320 s.
[0030] Example 5. In the method for selective leaching of copper and enrichment of precious metals by microwave treatment of carbonylation tailings according to any one of Examples 1-4, the atmospheric pressure leaching sulfuric acid concentration in step c) is 60-200 g / L, the leaching temperature is 70-95°C, the leaching time is 4-6 h, and the leaching liquid-to-solid ratio is 9-15:1.
[0031] Example 6. In the method for selective leaching of copper and enrichment of precious metals by microwave treatment of carbonylation tailings according to any one of Examples 1-5, the atmospheric pressure leaching sulfuric acid concentration in step c) is 180 g / L, the leaching temperature is 85°C, the leaching time is 5 h, and the leaching liquid-to-solid ratio is 12:1.
[0032] Example 7. In the method for selective leaching of copper and enrichment of precious metals by microwave treatment of carbonylation tailings according to any one of Examples 1 to 6, the amount of sulfuric acid used in the pressurized reduction leaching in step d) is 0.8 to 1.2 times the theoretical amount of nickel leached, the leaching temperature is 130 to 150°C, the leaching time is 2 to 6 hours, the leaching liquid-to-solid ratio is 6 to 10:1, and the sulfur dioxide partial pressure is 0.1 to 0.3 MPa.
[0033] Example 8. In the method for selective leaching of copper and enrichment of precious metals by microwave treatment of carbonylation tailings according to any one of Examples 1-7, the amount of sulfuric acid used in the pressurized reduction leaching in step d) is 1 times the theoretical amount of nickel leached, the leaching temperature is 140°C, the leaching time is 4h, the leaching liquid-to-solid ratio is 8:1, and the sulfur dioxide partial pressure is 0.2MPa.
[0034] Example 9: The mass percentages of the main elements in the carbonylation tailings of this example are shown in Table 1.
[0035] Table 1 Main element content of carbonylation tailings in Example 1 (%)
[0036]
[0037] Specific implementation process:
[0038] 1) Grind the carbonylation tailings and screen them to a particle size of -150 mesh.
[0039] 2) Add the ground carbonylation tailings into a microwave rotary kiln with a power of 6 kW and a microwave time of 540 s;
[0040] 3) adding the microwave carbonylation tailings into a beaker for leaching at normal pressure, controlling the leaching temperature to 70° C., the leaching time to 6 hours, the liquid-to-solid ratio to 9:1, and the sulfuric acid concentration to 200 g / L; after the reaction is completed, solid-liquid separation is performed to obtain a leaching solution and a leaching residue;
[0041] 4) Add the atmospheric pressure leaching residue into the autoclave, control the liquid-solid ratio to 6:1, the amount of sulfuric acid used is 1.0 times the theoretical amount of leached nickel, the leaching temperature is 150° C., the reaction time is 2 h, the sulfur dioxide partial pressure is 0.3 MPa, and after the reaction is completed, the solid-liquid separation is performed to obtain nickel sulfate leaching solution and precious metal enriched slag.
[0042] Table 2 Main output components of Example 1
[0043]
[0044] Example 10: The mass percentages of the main elements in the carbonylation tailings of this example are shown in Table 3.
[0045] Table 3 Main element contents of carbonylation tailings in Example 2 (%)
[0046]
[0047] Specific implementation process:
[0048] 1) Grind the carbonylation tailings and screen them to a particle size of -170 mesh.
[0049] 2) Add the carbonylation tailings in Table 3 into a microwave rotary kiln with a power of 8 kW and a microwave time of 480 s;
[0050] 3) adding the microwave carbonylation tailings into a beaker for leaching at normal pressure, controlling the leaching temperature to 80° C., the leaching time to 5 hours, the liquid-to-solid ratio to 10:1, and the sulfuric acid concentration to 150 g / L; after the reaction is completed, solid-liquid separation is performed to obtain a leaching solution and a leaching residue;
[0051] 4) Add the atmospheric pressure leaching residue into the autoclave, control the liquid-solid ratio to 8:1, the amount of sulfuric acid used is 1.2 times the theoretical amount of leached nickel, the leaching temperature is 130° C., the reaction time is 6 h, the sulfur dioxide partial pressure is 0.1 MPa, and after the reaction is completed, the solid-liquid separation is performed to obtain nickel sulfate leaching solution and precious metal enriched slag.
[0052] Table 4 Main output components of Example 2 (%)
[0053]
[0054] Example 11. The mass percentages of the main elements in the carbonylation tailings of this example are shown in Table 5.
[0055] Table 5 Main element contents of carbonylation tailings of Example 3 (%)
[0056]
[0057] Specific implementation process:
[0058] 1) Grind the carbonylation tailings and screen them to a particle size of -180 mesh.
[0059] 2) Add the carbonylation tailings in Table 5 into a microwave rotary kiln with a power of 9 kW and a microwave time of 240 s;
[0060] 3) adding the microwave carbonylation tailings into a beaker for leaching at normal pressure, controlling the leaching temperature to 90° C., the leaching time to 4 hours, the liquid-solid ratio to 11:1, and the sulfuric acid concentration to 80 g / L; after the reaction is completed, solid-liquid separation is performed to obtain a leaching solution and a leaching residue;
[0061] 4) Add the atmospheric pressure leaching residue into the autoclave, control the liquid-solid ratio to 10:1, the amount of sulfuric acid used is 0.8 times the theoretical amount of leached nickel, the leaching temperature is 140° C., the reaction time is 5 h, the sulfur dioxide partial pressure is 0.2 MPa, and after the reaction is completed, the solid-liquid separation is performed to obtain nickel sulfate leaching solution and precious metal enriched slag.
[0062] Table 6 Main output components of Example 3 (%)
[0063]
[0064]
[0065] Example 12. The mass percentages of the main elements in the carbonylation tailings of this example are shown in Table 7.
[0066] Table 7 Main element contents of carbonylation tailings of Example 4 (%)
[0067]
[0068] Specific implementation process:
[0069] 1) Grind the carbonylation tailings and screen them to a particle size of -200 mesh.
[0070] 2) Add the carbonylation tailings in Table 7 into a microwave rotary kiln with a power of 10 kW and a microwave time of 90 s;
[0071] 3) adding the microwave carbonylation tailings into a beaker for leaching at normal pressure, controlling the leaching temperature to 95° C., the leaching time to 4 hours, the liquid-to-solid ratio to 15:1, and the sulfuric acid concentration to 60 g / L; after the reaction is completed, solid-liquid separation is performed to obtain a leaching solution and a leaching residue;
[0072] 4) Add the atmospheric pressure leaching residue into the autoclave, control the liquid-solid ratio to 8:1, the amount of sulfuric acid used is 1.1 times the theoretical amount of leached nickel, the leaching temperature is 150° C., the reaction time is 2 h, the sulfur dioxide partial pressure is 0.2 MPa, and after the reaction is completed, the solid-liquid separation is performed to obtain nickel sulfate leaching solution and precious metal enriched slag.
[0073] Table 8 Main output components of Example 4 (%)
[0074]
[0075] The above is only a preferred embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solution and invention concept of the present invention within the scope disclosed by the present invention, which shall fall within the protection scope of the present invention.
Claims
1. A method for selectively leaching copper and enriching precious metals by microwave treatment of carbonylation tailings, characterized in that: The following steps are involved: a) Grinding: The carbonylation tailings are ground and the particle size is controlled at -150 to -200 mesh; b) microwave treatment: adding the carbonylation tailings obtained in step a) into a microwave rotary kiln for microwave pretreatment; c) Sulfuric acid leaching: subjecting the microwave-treated carbonylation tailings obtained in step b) to leaching with sulfuric acid at normal pressure, and after the reaction is completed, solid-liquid separation is performed to obtain copper sulfate leaching solution and nickel-containing precious metal leaching residue; d) pressure reduction leaching: the nickel-containing precious metal leaching residue obtained in step c) is subjected to pressure reduction leaching, and after the reaction is completed, the solid-liquid separation is performed to obtain the nickel-containing leaching solution and the precious metal-enriched residue.
2. The method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to claim 1, characterized in that: The carbonylation tailings are obtained by carbonylating an alloy obtained by a magnetic separation process to produce carbonyl nickel from high-grade nickel matte obtained by pyrometallurgical iron blowing of nickel-copper sulfide ore.
3. The method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to claim 1, characterized in that: In the step b), the microwave pretreatment is performed with a power of 6 kW to 10 kW and a microwave time of 90 to 540 s.
4. The method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to claim 3, characterized in that: In the step b), the microwave pretreatment is performed with a controlled power of 8 kW and a microwave time of 320 s.
5. The method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to claim 1, characterized in that: In the step c), the concentration of sulfuric acid in the atmospheric pressure leaching is 60-200 g / L, the leaching temperature is 70-95° C., the leaching time is 4-6 hours, and the leaching liquid-to-solid ratio is 9-15:
1.
6. The method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to claim 5, characterized in that: In the step c), the atmospheric pressure leaching sulfuric acid concentration is 180 g / L, the leaching temperature is 85° C., the leaching time is 5 h, and the leaching liquid-to-solid ratio is 12:
1.
7. The method for realizing copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to claim 1, characterized in that: In the step d), the amount of sulfuric acid used for pressurized reduction leaching is 0.8 to 1.2 times the theoretical amount of nickel leached, the leaching temperature is 130 to 150° C., the leaching time is 2 to 6 hours, the leaching liquid-to-solid ratio is 6 to 10:1, and the sulfur dioxide partial pressure is 0.1 to 0.3 MPa.
8. The method for achieving copper selective leaching and precious metal enrichment by microwave treatment of carbonylation tailings according to claim 7, characterized in that: In the step d), the amount of sulfuric acid used for pressurized reduction leaching is 1 times the theoretical amount of nickel leached, the leaching temperature is 140° C., the leaching time is 4 hours, the leaching liquid-to-solid ratio is 8:1, and the sulfur dioxide partial pressure is 0.2 MPa.
Citation Information
Patent Citations
Process of recovering noble metal from hydroxylating metallurgy slag
CN100999784A
Method for treating carbonylation slag
CN117210690A
Process for synthesizing nickel carbonyl under normal pressure
CN1951826A
Roast-reductive leach process for copper recovery
US4135918A
Roast-leach copper recovery
US4168217A