Preparation method for capturing platinum group noble metal in automobile waste catalyst by jamesonite
By decomposing brittle sulfhydryl lead antimony ore into sulfide trapping agent, combining slag-making agent, vacuum distillation and hydrometallurgy processes, the limitations of high-temperature smelting and pure metal trapping agents in the existing technology are solved, and platinum is achieved High-efficiency recycling and environmentally friendly recycling processes for family precious metals.
Patent Information
- Application Number
- CN202410971880.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, when recovering platinum group precious metals from waste automobile catalysts, the commonly used fire process is limited by high-temperature smelting and pure metal trapping agents, resulting in complex processes and environmental pollution, and it is difficult to effectively utilize brittle sulfur lead antimony ore. Precious metal resources.
By decomposing brittle sulfhydryl lead antimony ore into Sb2S3, PbS and FeS, a sulfide trapping agent is formed, and combined with slag-making agents such as B2O3, Na2O or SiO2, vacuum distillation and hydrometallurgy processes are used to achieve efficient capture of platinum group precious metals. Collect and separate, avoiding the use of pure metal trapping agents.
It realizes efficient recycling of platinum group precious metals, reduces process complexity and environmental pollution, simplifies the process, and utilizes cheap brittle sulfur lead antimony ore resources, improving the recovery rate and process feasibility.
Smart Images

Figure CN118910419A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nonferrous metal smelting, and in particular to a preparation method for capturing platinum group precious metals in automobile waste catalysts by using brittle sulfur lead antimony ore. Background Art
[0002] Waste automobile catalysts (SACs) are an important secondary resource of platinum group metals. Recovering platinum group metals from waste catalyst secondary resources is of great significance to solving the serious shortage of platinum group metal mineral resources in my country and ensuring the safe and stable supply of platinum group metals. The commonly used methods for recovering platinum group metals from waste automobile exhaust catalysts can be divided into wet recovery and pyrometallurgical recovery. The current mainstream process in the industry is the pyrometallurgical process, which uses non-precious metals to mix waste catalysts with slag-forming agents and metal collectors and then smelt them at high temperatures. The oxides in the system form slag, and the platinum group metals enter the metal phase together with the metal to form an alloy to achieve the purpose of enrichment. Commonly used collectors in the industry include iron, lead, copper, nickel matte, etc.
[0003] Matte capture of precious metals mainly includes nickel matte, iron sulfur and copper matte. Nickel matte captures platinum group metals in waste automobile exhaust catalysts. Under the optimized conditions of 3.5 silica content, 0.88g nickel, 0.98g sulfur, 1.33g sodium carbonate, 2.67g borax and 1050℃ smelting for 30min, the detection recovery rates of Pt, Pd and Rh are 99.50%, 98.07% and 98.99% respectively. Morca li uses iron matte to capture platinum group metals in waste catalysts. 50g waste catalyst, 150g solvent (NaO:B2O3=1:0.6-0.8) and 10g FeS2 are mixed and smelted at 950℃ for 75min. Platinum group metals can be enriched 6 times, and the recovery rates of Pt, Pd and Rh are 99%, 99% and 97% respectively. Matte smelting has a high recovery rate for capturing precious metals, and can be combined with smelting enterprises and easily industrialized. Sulphurous lead antimony ore is a polymetallic sulfide that can be decomposed into Sb2S3, PbS and FeS after vacuum thermal decomposition. In addition, the mineral also contains FeS2. These sulfides can capture precious metals. The SiO2 contained in the mineral itself can also be used as a slag-making agent. Summary of the invention
[0004] (I) Technical solution
[0005] The present invention combines the advantages of metal sulfide capture of platinum group precious metals in catalysts and the characteristics of brittle sulfur lead antimony concentrate that can decompose Sb2S3, PbS and FeS, and is achieved through the following technical scheme: a preparation method for brittle sulfur lead antimony ore to capture platinum group precious metals in automobile waste catalysts, comprising the following steps:
[0006] (1) placing the brittle sulfur lead antimony concentrate in a vacuum furnace and heating it to a specified temperature to decompose it into Sb2S3, PbS and FeS. The mineral also contains some FeS2 and gangue SiO2;
[0007] (2) The three sulfides of Sb2S3, PbS and FeS are subjected to vacuum distillation, volatilization and graded condensation to obtain Sb2S3, PbS, FeS and FeS2 in the mineral respectively, leaving them in the residue.
[0008] (3) using the single sulfides Sb2S3, PbS, FeS and FeS2 in minerals obtained above, or mixed sulfides to form a sulfide collector, and adding B2O3, Na2O or SiO2, CaO slag-forming agents according to the melting point of the single sulfide or mixed sulfide, wherein the ratio of B2O3 to Na2O in the slag-forming agent is controlled to be 0.6-0.8, and the ratio of SiO2 to CaO is 0.4-0.8;
[0009] (4) If the collector is Sb2S3, PbS or a mixture, the platinum group precious metal enters the sulfide to form a matte containing precious metals, and then a vacuum distillation process is used to evaporate the excess sulfide and the lead and antimony in the matte to obtain the precious metals; if FeS and FeS2 in the mineral are used, a hydrometallurgical process is subsequently used, and after crushing, aqua regia is used to dissolve and remove the iron in the alloy to obtain the precious metals.
[0010] Preferably, the concentrate is heated under low temperature vacuum conditions to decompose it into different sulfides; the vacuum pressure is controlled at 1-10Pa.
[0011] Preferably, the waste catalyst is crushed to less than 200 meshes, and the mass addition ratio of the waste catalyst, the collector and the slag-forming agent is 1:(1.2-2):(2-3). In the above steps, the collector is first obtained from the concentrate by vacuum distillation, and then a single sulfide or a mixed sulfide is used to form a single lead matte or lead antimony matte as a collector, and B2O3, Na2O or SiO2, CaO are used as slag-forming and solvents, which have the functions of mass transfer and heat transfer, transfer of electrons, and assisting in melting the carrier cordierite in the catalyst, forming a slag phase that is conducive to separation.
[0012] Preferably, during the reaction in step (1), the reaction temperature is controlled to be 400-600°C, the reaction time is 1-4h, and the heating rate is 5-10°C / min.
[0013] Preferably, when Sb2S3 and PbS are used as collectors in step (3), the ratio of PbS to Sb2S3 is (2-5):1, the smelting temperature is 800-1000°C, and precious metal-Pb-Sb-S is obtained after smelting, and in step (4), a vacuum distillation method is used to separate precious metals and sulfides, the vacuum distillation temperature is 600-800°C, and the pressure is 5-30Pa.
[0014] Preferably, when FeS2 or FeS is used as a collector in step (3), the mass addition ratio of the waste catalyst, the collector and the slag-forming agent is 1:(1.2-2):(3-5), the smelting temperature is 1000-1200°C, and the precious metal-Fe-S is obtained after smelting. In step (4), hydrometallurgy is used to separate the precious metal and the sulfide, and the leaching reagent is selected from one or more mixtures of sulfuric acid, hydrochloric acid and aqua regia.
[0015] Preferably, the distillation temperature of the argon atmosphere furnace is 1000-1200°C, the time is 2-4h, the heating rate is 5-10°C / min, and the pressure is 5-30Pa;
[0016] Preferably, the distillation temperature in the vacuum distillation process in step (4) is 800-1000°C, the time is 2-4h, the heating rate is 5-10°C / min, and the pressure is 5-30Pa.
[0017] (II) Beneficial effects
[0018] The present invention provides a preparation method for capturing platinum group precious metals in automobile waste catalysts using brittle sulfide lead antimony ore. It has the following beneficial effects:
[0019] The present invention avoids using pure metal as a collector, avoids the drawback of high melting temperature of pure metal as a collector, and uses three sulfides of lead, antimony and iron as collectors. Moreover, the sulfides of the present invention all come from very cheap brittle sulfur lead antimony concentrate, and the three sulfides decomposed from the brittle sulfur lead antimony ore can all be used as precious metal collectors, achieving the purpose of mineral capture of precious metals. At the same time, the lead antimony matte capture process of the present invention reduces the hydrometallurgical process, and uses vacuum distillation to treat the lead antimony matte containing precious metals, which has the characteristics of low environmental pollution and simple and easy operation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The present invention is a schematic diagram of the process flow of the method for capturing automobile exhaust waste catalyst platinum group precious metals with brittle sulfur lead antimony concentrate. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Embodiment 1:
[0023] like Figure 1 As shown, the preparation method of brittle sulfide lead antimony ore to capture platinum group precious metals in automobile waste catalysts comprises the following steps:
[0024] (1) The brittle sulfur lead antimony concentrate is placed in a vacuum furnace, and the pressure in the furnace is reduced to 10 Pa by a vacuum pump. The vacuum furnace is heated to raise its temperature to 500°C, and the brittle sulfur lead antimony concentrate is decomposed into PbS, Sb2S3 and FeS. Then, a graded condensation device is used to separate PbS, Sb2S3 and FeS. PbS and Sb2S3 are condensed and enriched in different condensation plates, and FeS remains in the residue and is mixed with FeS2 in the concentrate, i.e., pyrite.
[0025] (2) Automobile exhaust waste catalyst, PbS and Sb2S3, B2O3 and Na2O powder, wherein the molar ratio of PbS to Sb2S3 is 4:1, the mass ratio of B2O3 to Na2O powder is 0.7, and automobile exhaust waste catalyst, PbS and Sb2S3, B2O3 and Na2O powder are mixed in a mass ratio of 1:1.8:2.5 to obtain a mixture, and argon is introduced into an atmosphere furnace to increase the temperature to 1000°C at a heating rate of 6°C / min, and the temperature is kept for 2 hours. After the insulation is completed, the heating is stopped, and after the atmosphere furnace is naturally cooled to less than 50°C, a first-stage smelting product is obtained.
[0026] (3) The matte containing platinum group precious metals in the smelting product is taken out and separated from the slag. The atmosphere furnace is evacuated to a vacuum degree of 10 Pa, and the temperature is raised to 900°C and kept warm for 1 hour to volatilize the lead antimony sulfide in the matte to obtain platinum group precious metals Pt, Pd, and Rh residues. After analysis, the capture rates of platinum and palladium can reach more than 98%, and the capture rate of rhodium is about 93%.
[0027] The composition of platinum group precious metals in the automobile exhaust waste catalyst in this embodiment is: Pt mass content is 122g / t, Pd is 1015g / t, and Rh is 148g / t. The mass fractions of lead, antimony, iron and sulfur in the brittle sulfur lead antimony concentrate are 22.3%, 18%, 14.2% and 26.4% respectively.
[0028] Embodiment 2:
[0029] like Figure 1As shown, the preparation method of brittle sulfide lead antimony ore to capture platinum group precious metals in automobile waste catalysts comprises the following steps:
[0030] (1) The brittle sulfur lead antimony concentrate is placed in a vacuum furnace, and the pressure in the furnace is reduced to 5 Pa by a vacuum pump. The vacuum furnace is heated to raise its temperature to 480°C, and the brittle sulfur lead antimony concentrate is decomposed into PbS, Sb2S3 and FeS. Then, a graded condensation device is used to separate PbS, Sb2S3 and FeS. PbS and Sb2S3 are condensed and enriched in different condensation plates, and FeS remains in the residue and is mixed with pyrite in the concentrate, i.e., FeS2.
[0031] (2) Waste catalyst from automobile exhaust, FeS2 or FeS, B2O3 and Na2O powder are mixed uniformly in a mass ratio of 1:1.5:3 to obtain a mixture, wherein the mass ratio of B2O3 to Na2O powder is 0.65, and argon is introduced into the atmosphere furnace to increase the temperature to 1200°C at a heating rate of 6°C / min, and the temperature is kept for 2 hours. After the temperature is kept, the heating is stopped, and the atmosphere furnace is cooled naturally to less than 50°C to obtain a first-stage smelting product.
[0032] (3) The smelting product is leached with a mixed solution of hydrochloric acid and hydrogen peroxide to remove Fe in the matte, and finally the platinum group precious metals are obtained. After analysis, the capture rates of platinum and palladium can reach more than 98%, and the capture rate of rhodium is about 93%.
[0033] In this embodiment, the composition of platinum group precious metals in the automobile exhaust waste catalyst is: Pt mass content is 122g / t, Pd is 1015g / t, and Rh is 148g / t. The mass fractions of lead, antimony, iron and sulfur in the brittle sulfur lead antimony concentrate are 22.3%, 18%, 14.2% and 26.4% respectively. The hydrochloric acid concentration is 6mol / L, the amount of hydrogen peroxide added is 40Ml / L, and the leaching temperature is 80℃.
[0034] Embodiment three:
[0035] (1) The brittle sulfur lead antimony concentrate is placed in a vacuum furnace, and the pressure in the furnace is reduced to 1 Pa by a vacuum pump. The vacuum furnace is heated to raise its temperature to 450°C, and the brittle sulfur lead antimony concentrate is decomposed into PbS, Sb2S3 and FeS. Then, a graded condensation device is used to separate PbS, Sb2S3 and FeS. PbS and Sb2S3 are condensed and enriched in different condensation plates, and FeS remains in the residue and is mixed with pyrite in the concentrate, i.e., FeS2.
[0036] (2) Waste catalyst from automobile exhaust, PbS and Sb2S3, SiO2 and CaO powders are mixed uniformly in a mass ratio of 1:1.6:3 to obtain a mixture, wherein the molar ratio of PbS to Sb2S3 is 4:1, and the mass ratio of SiO2 to CaO powder is 0.7. Argon is introduced into an atmosphere furnace and the temperature is raised to 1000°C at a heating rate of 6°C / min. The temperature is kept for 2 hours. After the temperature is kept, the heating is stopped, and after the atmosphere furnace is naturally cooled to less than 50°C, a first-stage smelting product is obtained.
[0037] (3) The matte containing platinum group precious metals in the smelting product is taken out and separated from the slag. The atmosphere furnace is evacuated to a vacuum degree of 10 Pa, and the temperature is raised to 900°C and kept warm for 1 hour to volatilize the lead antimony sulfide in the matte to obtain platinum group precious metals Pt, Pd, and Rh residues. After analysis, the capture rates of platinum and palladium can reach more than 98%, and the capture rate of rhodium is about 94%.
[0038] The composition of platinum group precious metals in the automobile exhaust waste catalyst in this embodiment is: Pt mass content is 122g / t, Pd is 1015g / t, and Rh is 148g / t. The mass fractions of lead, antimony, iron and sulfur in the brittle sulfur lead antimony concentrate are 22.3%, 18%, 14.2% and 26.4% respectively.
[0039] That is, in the above embodiment, the first step is vacuum distillation of brittle sulfur lead antimony concentrate, the second step is volatilization and fractionation condensation to obtain sulfides such as Sb2S3, PbS, FeS and FeS2, and the third step is to use lead antimony matte or iron sulfur to capture platinum group precious metals in waste automobile catalysts, wherein the melting point of lead antimony matte changes according to the different proportions of added lead sulfide and antimony sulfide, and a relatively low melting point and non-volatile proportion is selected to form lead antimony matte as a collector; iron sulfur can also be used as a collector to capture platinum group precious metals in catalysts. If lead antimony matte is used for capture, the precious metals enter the lead antimony matte, and the vacuum distillation process is further used to remove lead and antimony to obtain the precious metals; if FeS2 and FeS are used, the precious metals enter the iron matte, and then the hydrometallurgical process is used to separate iron and precious metals. It has the characteristics of low environmental pollution and simple and easy operation.
[0040] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing platinum group precious metals from automobile waste catalysts by using brittle sulfide lead antimony ore, characterized in that: The following steps are involved: Step (1). The brittle sulfur lead antimony concentrate is placed in a vacuum furnace, the vacuum pressure is controlled at 1-10Pa, and decomposed into three sulfides Sb2S3, PbS, and FeS under vacuum conditions. The reaction temperature is 400-600°C, the time is 1-4h, and the heating rate is 5-10°C / min. Sb2S3 and PbS are obtained by fractional condensation using a decomposition and condensation device, and FeS and FeS2 and SiO2 in the concentrate are left in the residue; Step (2) the step (1) obtained in the sulfide Sb2S3, PbS, FeS or FeS2 in one or more mixtures as automobile exhaust waste catalyst platinum group precious metal capture agent; Step (3) the platinum group metal collector in step (2) and the waste catalyst, slag agent uniformly mixed, heated in an argon atmosphere furnace for a two-stage smelting reaction, to obtain a precious metal-containing matte and slag phase; Step (4). The second-stage smelting product in step (3) is subjected to vacuum distillation separation and wet separation method selection according to the type of selected platinum group metal capture agent, and finally the platinum group precious metals Pt, Pd, and Rh are obtained.
2. The method for preparing platinum group noble metals from automobile waste catalysts by using brittle sulfide lead antimony ore according to claim 1, characterized in that: In the step (3), when the automobile exhaust waste catalyst and Sb2S3 and PbS or FeS and FeS2 collector powders are evenly mixed, B2O3, Na2O or SiO2, CaO slag-forming agents are also added; the waste catalyst powder is ball-milled to a particle size of less than 200 mesh, the ratio of B2O3 to Na2O is 0.6-0.8:1, and the ratio of SiO2 to CaO is 0.6-1:
1.
3. The method for preparing platinum group noble metals from automobile waste catalysts by using brittle sulfide lead antimony ore according to claim 1, characterized in that: The mass addition ratio of the waste catalyst, the collector and the slag-forming agent is: 1:(1.2-2):(2-3).
4. The method for preparing platinum group noble metals from automobile waste catalysts by using brittle sulfide lead antimony ore according to claim 1, characterized in that: When Sb2S3 and PbS are used as collectors in step (3), the ratio of PbS to Sb2S3 is (2-5):1, the smelting temperature is 800-1000°C, and precious metal-Pb-Sb-S is obtained after smelting. In step (4), a vacuum distillation method is used to separate precious metals and sulfides, the vacuum distillation temperature is 600-800°C, and the pressure is 5-30Pa.
5. The method for preparing platinum group noble metals from automobile waste catalysts by using brittle sulfide lead antimony ore according to claim 1, characterized in that: When FeS2 or FeS is used as a collector in the step (3), the mass addition ratio of the waste catalyst, the collector and the slag-forming agent is 1:(1.2-2):(3-5), the smelting temperature is 1000-1200°C, and the precious metal-Fe-S is obtained after smelting. In the step (4), hydrometallurgy is used to separate the precious metal and the sulfide, and the leaching reagent is selected from one or more mixtures of sulfuric acid, hydrochloric acid and aqua regia.
6. The method for preparing platinum group noble metals from automobile waste catalysts by using brittle sulfide lead antimony ore according to claim 1, characterized in that: The temperatures for decomposition and vacuum volatilization of the brittle lead antimonite are 400-600° C. and 1000-1200° C., respectively, and the pressure is 5-30 Pa.