Manufacturing method of tungsten-containing alloy target material
By mixing the elements to be synthesized with the tungsten element particles and sintering and crushing during the target preparation process, the problem of difficulty in controlling the proportion of light metals and heavy metals is solved, the stability and uniformity of the composite layer are achieved, and the composite coating is ensured. stability and consistency.
Patent Information
- Application Number
- CN202410988375.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, during the preparation of the target material of a multi-component coating material, the ratio of light metals and heavy metals is difficult to control, resulting in poor stability of the composite coating and uneven element distribution.
By mixing the elements to be synthesized with the tungsten element particles and grinding to 3 to 5 microns, performing initial sintering and coarse pulverization, followed by sintering using a hot isostatic vacuum envelope, the sintering temperature is 0.7 to 0.9 times the melting temperature of the most element content. Ensure uniformity and stability of element proportions.
The uniformity and stability of the element ratio in the composite target material is achieved, ensuring the stability and consistency of the subsequent composite layer.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor target materials, and in particular to a method for manufacturing a tungsten-containing alloy target material. Background Art
[0002] Physical vapor deposition (PVD) technology refers to the technology of using physical methods to deposit a thin film with special functions on the surface of a substrate by vaporizing a material source (solid or liquid surface is vaporized into gaseous atoms, molecules or partially ionized into ions) under vacuum conditions through a low-pressure gas (or plasma) process. The main methods of physical vapor deposition include vacuum evaporation, sputtering, arc plasma plating, ion plating, and molecular beam epitaxy. Physical vapor deposition technology can not only deposit metal films and alloy films, but also compounds, ceramics, semiconductors, polymer films, etc.
[0003] Due to the development of physical vapor deposition coating technology, it is widely used on the surface of tools / molds, making the structure and elements of the surface coating more complex, especially the diversity of elements, which has developed from the original single metal to binary metal, ternary metal, and even metal and non-metal composites.
[0004] Multi-component composite coating materials require composite targets of multiple metal elements. In order to achieve diversity in composite coatings, light metals such as aluminum and titanium or non-metals such as silicon, as well as heavy metals such as tungsten are often used. Due to the large ratio of light metals to heavy metals and the large difference in melting temperatures, it is often used to prepare the target material with the light metal first and then prepare the heavy metal or non-metal into separate blocks and embed them into the light metal target material. The target material prepared in this way cannot guarantee the etching rate of the composite coating, and it will also make the proportion of deposited elements difficult to control, mainly referring to the uneven proportion, which leads to poor stability of the composite coating. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a tungsten-containing alloy target material. The alloy ratio of the composite target material prepared by the method is uniform, so that the ratio between various elements is relatively stable at any position of the target material.
[0006] To achieve the above purpose, the present invention adopts the following technical solutions:
[0007] A method for manufacturing a tungsten-containing alloy target comprises the following steps:
[0008] (1) Selecting particles of the element to be synthesized and particles of tungsten element to mix, and further grinding the mixed particles until the particle size is 3 to 5 microns;
[0009] (2) The ground particles are initially sintered at a temperature equal to the melting point of the element with the lowest content in the mixed particles for 130 min; after sintering, the particles are cooled to room temperature;
[0010] (3) coarsely crushing the alloy after the initial sintering, wherein the particle size of the crushed particles is 6 to 13 times the particle size of the particles in step (1);
[0011] (4) hot isostatic pressing vacuum envelope sintering is performed on the coarsely crushed alloy according to the target blank, the sintering temperature is 0.7 to 0.9 times the melting temperature of the element with the highest content in the mixed particles, and the sintering time is 180 minutes; after sintering, fine processing is performed to produce the alloy target.
[0012] Furthermore, inert gas is introduced into the particles during the mixing process in step (1).
[0013] Furthermore, the grinding in step (1) is performed by ball milling technology, and an inert gas is filled during the ball milling process.
[0014] Furthermore, the inert gas is high-purity argon or helium.
[0015] Furthermore, the particle size of the coarsely crushed particles in step (3) is 35 to 55 microns.
[0016] The present invention uses the cooling process of the metal after melting as a binder for other metals through mixed initial sintering, so that the particles are fully mixed to ensure the uniformity, consistency and stability of the material, thereby ensuring the stability, uniformity and consistency of the composite layer prepared subsequently. DETAILED DESCRIPTION
[0017] Example 1
[0018] The present embodiment provides a method for producing a tungsten-containing alloy target material. The method of the present embodiment is described in detail by taking aluminum, chromium, and silicon elements as examples. The preparation schemes for other composite elements are similar, and only the sintering temperature and time involved in the steps are changed according to the melting temperature of the elements, and other general steps remain unchanged.
[0019] Preparation method:
[0020] (1) Take 100g of aluminum powder with a theoretical purity of ≥98%, 200g of chromium powder, 150g of tungsten powder and 120g of polycrystalline silicon particles with a mass fraction of 28.43-29.96wt.%, mix the aluminum powder, chromium powder, tungsten powder and polycrystalline silicon particles and put them into a ball mill for grinding. Inert gas is filled in the grinding process to prevent the aluminum powder (light metal) from spontaneously igniting due to contact with oxygen and grinding heat during the grinding process. The inert gas is high-purity helium or argon. Grind until the particle size is 3-5 microns.
[0021] (2) The ground mixed particles are placed on a placing plate, spread evenly, and then sent into a vacuum sintering furnace for initial sintering. The sintering temperature is the melting temperature of the element with the lowest content in the mixed particles. The melting temperature of aluminum powder is 660°C; the melting temperature of chromium powder is 1857°C; the melting temperature of tungsten powder is 3390°C~3430°C; the melting temperature of polysilicon particles is 1410°C. Therefore, the sintering temperature of this embodiment is controlled at about 660°C, and the sintering time is 130 minutes. During the sintering process, the aluminum powder is melted and acts as an adhesive to bond heavy metals and non-metals. After sintering, the powder is cooled to room temperature. In this process, the element distribution of the solidified powder can be scraped off to ensure that the element distribution of the target material prepared later is uniform.
[0022] (3) The alloy ingot formed by the initial sintering and cooling to room temperature is crushed, and the crushed particles are larger than the particle size of the particles after ball milling in step (1), specifically 6 to 13 times the particle size of the particles after ball milling. In this embodiment, it is controlled to be 35 to 55 microns. The crushed particles are then mixed to further achieve sufficient mixing of various elements, thereby ensuring uniform distribution of elements in the later target material.
[0023] (4) The mixed alloy particles in step (3) are subjected to hot isostatic pressing vacuum sealing according to the target blank, specifically, the mixed particles are filled into a rubber sleeve of a mold, and then the rubber sleeve is sealed and evacuated, and the evacuated rubber sleeve is placed on a cold isostatic press, and an initial pre-pressing is performed at a pressure of 20 to 50 MPa to form a rough blank, and the obtained rough blank is subjected to secondary pressing at a pressure of 150 to 200 MPa until the density of the green blank reaches 60 to 62% of the theoretical density, and the pressure is released to normal pressure.
[0024] (5) A green embryo with a theoretical density of 60 to 62% is placed in a vacuum hot pressing sintering furnace and hot pressed at a pressure of 120 to 160 MPa. The sintering temperature is 0.7 to 0.9 times the melting temperature of the element with the highest content in the mixed elements. The sintering temperature of this embodiment is 750 to 800° C. and the sintering time is 180 min. After sintering, the vacuum envelope is removed and cooled to room temperature to obtain a crude alloy target material. The crude alloy target material is then finely processed according to parameters such as the size of the target material to obtain the alloy target material.
[0025] The target material of this embodiment is used to prepare the composite layer, and the uniformity of the element distribution of the composite layer is tested, and the uniformity of the element distribution of the composite layer prepared by the prior art is tested.
[0026] The above description is only a preferred implementation manner of the present invention, but the protection scope of the present invention is not limited thereto, and any modification and replacement based on the technical solution and inventive concept provided by the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing a tungsten-containing alloy target, characterized in that The steps include: (1) Selecting particles of the element to be synthesized and particles of tungsten element to mix, and further grinding the mixed particles until the particle size is 3 to 5 microns; (2) The ground particles are initially sintered at a temperature equal to the melting point of the element with the lowest content in the mixed particles for 130 min; after sintering, the particles are cooled to room temperature; (3) coarsely crushing the alloy after the initial sintering, wherein the particle size of the crushed particles is 6 to 13 times the particle size of the particles in step (1); (4) hot isostatic pressing vacuum envelope sintering is performed on the coarsely crushed alloy according to the target blank, the sintering temperature is 0.7 to 0.9 times the melting temperature of the element with the highest content in the mixed particles, and the sintering time is 180 minutes; after sintering, fine processing is performed to produce the alloy target.
2. The method for producing a tungsten-containing alloy target according to claim 1, characterized in that: In the mixing process in step (1), an inert gas is introduced into the particles.
3. The method for producing a tungsten-containing alloy target according to claim 2, characterized in that: The grinding in step (1) is performed by ball milling technology, and an inert gas is filled during the ball milling process.
4. The method for producing a tungsten-containing alloy target according to claim 3, characterized in that: The inert gas is high-purity argon or helium.
5. The method for producing a tungsten-containing alloy target according to claim 1, characterized in that: The particle size of the coarsely crushed particles in step (3) is 35 to 55 microns.