Discharge plasma liquid phase sintering preparation method of high-density LaB6-Ni composite material

By introducing trace amounts of Ni during LaB6 sintering, and using discharge plasma liquid phase sintering technology, the problems of low sintering activity and high temperature of LaB6 are solved, and a high density and excellent performance LaB6-Ni composite material is prepared, achieving energy saving and Effects of industrialization.

CN118910452APending Publication Date: 2024-11-08HEFEI UNIV OF TECH

Patent Information

Application Number
CN202411407426.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The problems of low activity and high sintering temperature in the existing LaB6 sintering technology lead to long sintering time and large energy consumption, making it difficult to prepare high-density polycrystalline materials.

Method used

A trace amount of low-melting point metal Ni is introduced, and the discharge plasma liquid phase sintering technology is used to form a liquid phase as Ni increases with the sintering temperature, wetting the LaB6 powder particles, significantly reducing the sintering temperature and time, and preparing a high-density LaB6-Ni composite material.

Benefits of technology

LaB6-Ni composite materials with high density, excellent hardness and thermal electron emission performance are energy-saving and suitable for industrial production and applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910452A_ABST
    Figure CN118910452A_ABST
Patent Text Reader

Abstract

The invention provides a spark plasma liquid phase sintering preparation method of a high-density LaB6-Ni composite material, and relates to the technical field of rare earth hexaboride cathode materials. Comprising the steps that a trace amount of low-melting-point metal Ni second phase is introduced, metal Ni forms a liquid phase along with rising of the sintering temperature in the spark plasma sintering process, LaB6 powder particles are wetted, the sintering temperature is remarkably reduced, the sintering time is remarkably shortened, and the LaB6-Ni composite material is prepared through spark plasma liquid phase sintering. After weighing, ball milling, drying and pre-pressing molding, the material is prepared by adopting a spark plasma liquid phase sintering technology. The material is high in density, high in hardness and excellent in thermionic emission performance, and the method saves energy and cost and is suitable for industrial production and application of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth hexaboride cathode materials, and specifically relates to a method for preparing a high-density LaB6-Ni composite material by spark plasma liquid phase sintering. Background Art

[0002] Lanthanum hexaboride (LaB6) is an excellent hot cathode material with high melting point, high hardness, low work function and good chemical stability. It is widely used in various high-resolution electronic analysis instruments, electron beam welders and high-energy accelerators. With the rapid development of my country's deep space exploration and high-power and high-frequency vacuum electronic devices, new research and development requirements for hot cathode materials have been put forward. High-density polycrystalline LaB6 blocks can meet the needs of high-current and long-life hot cathode devices, so how to prepare high-density polycrystalline LaB6 is a key issue.

[0003] At present, the preparation technology of LaB6 polycrystals is mainly hot pressing and spark plasma sintering. Hot pressing sintering is a traditional material sintering technology. First, the powder is loaded into the mold, and then the mold is pressurized and heated at one end at the same time, so that the powder molding and sintering are completed together. The advantages of this method are simple preparation process, low cost and mature technology. However, in order to obtain highly densified sintered samples, hot pressing sintering often requires a high temperature and high pressure preparation environment, and also requires a long insulation time, which makes the sintered body grains very easy to grow. Gao Ruilan and others from Shandong University used this method to prepare LaB6 polycrystalline blocks. The specific process parameters are as follows: sintering temperature 2100 degrees, sintering pressure 50MPa, insulation 2h, and the sample density reached 92%.

[0004] Spark plasma sintering (SPS) is a new type of sintering method. It can generate spark discharge at the beginning of sintering by high current ON-OFF DC pulse power supply, which has the effect of purifying and activating the surface of powder particles; in the middle and late stages of sintering, Joule heat, thermal diffusion generated by electromagnetic energy and electric field interface diffusion are used to promote densification, and rapid sintering is achieved through self-heating and rapid heating inside the initial powder. The advantages of SPS technology are very obvious: uniform heating, low sintering temperature, fast heating rate, short sintering time, fine and uniform sample structure, and will not change the natural state of the original material. Compared with hot pressing sintering, SPS equipment is simple to operate, has higher safety performance, and the sintering temperature can generally be reduced by 100-200℃ or even higher. This research group used spark plasma solid phase sintering technology to prepare LaB6 polycrystalline blocks with a density of >97%. The process parameters are as follows: sintering temperature 1930℃, sintering pressure 45MPa, and insulation for 19min (Comparative Example 2). By comparison, spark plasma sintering can significantly reduce the sintering temperature and improve the density of the sample.

[0005] However, due to the stable BB covalent bond of LaB6, its atomic diffusion is very slow during the solid phase sintering process. It takes a long sintering time and a very high sintering temperature to obtain highly dense LaB6 polycrystals by hot pressing sintering or spark plasma solid phase sintering. Compared with solid phase sintering, liquid phase sintering can greatly promote particle aggregation and accelerate the sintering process through the wetting effect of the liquid phase formed during the sintering process on the surface of the powder particles, thereby significantly reducing the sintering temperature and sintering time. Summary of the invention

[0006] (I) Technical problems to be solved: In order to solve the problems of low sintering activity and high sintering temperature of LaB6 in the prior art, the present invention aims to provide a spark plasma liquid phase sintering method for preparing a high-density LaB6-Ni composite material.

[0007] (II) Technical solution: To solve the technical problem, the present invention adopts the following technical solution: By introducing a small amount of low-melting-point metal Ni second phase, during the spark plasma sintering process, the metal Ni forms a liquid phase as the sintering temperature increases, and then wets the LaB6 powder particles, significantly reducing the sintering temperature and sintering time, and finally obtaining a high-density LaB6-Ni composite material, that is, a spark plasma liquid phase sintering preparation method for a high-density LaB6-Ni composite material, which is characterized in that: LaB6 powder and metal Ni powder are used as raw materials, and after weighing, ball milling, drying, and pre-pressing, the LaB6-Ni composite material is prepared by spark plasma liquid phase sintering technology. The specific steps are as follows: (1) LaB6 powder and metal Ni powder are weighed and filled into cans according to different proportions, and then loaded into a powder mixer for mixing to obtain uniform powder.

[0008] (2) The mixed powder obtained in step (1) was placed in a stainless steel ball mill, and stainless steel balls were added as a ball milling medium at a ball-to-material ratio of 10:1. The ball mill was evacuated and then filled with argon (this process was repeated 3 times), and then placed in a high-energy ball mill for 8 hours at a ball milling frequency of 45 Hz.

[0009] (3) The ball-milled powder obtained in step (2) was placed in a vacuum drying oven and dried at 80°C for 12 h before being taken out.

[0010] (4) Place the dried powder into a graphite mold and wrap the powder with a thin carbon paper to isolate the graphite mold and the pressure head. Then pre-press the powder on a hydraulic press with a pre-pressure of 3MPa and place the powder in the middle of the mold. After the pre-pressing is completed, wrap a layer of carbon felt on the surface of the mold and place it in a spark plasma sintering furnace. Adjust the mold position through a graphite pad and connect the upper and lower electrodes of the sintering furnace to form a sintering current. Then evacuate to below 5Pa and start sintering. The process parameters are as follows: The sintering processes of LaB6-Ni composite materials formed by doping 0-4wt.% and 4-5wt.% Ni are different, as follows: LaB6-0-4wt.%Ni: The first stage: the sintering temperature is increased from room temperature to 1300℃, the heating rate is 80-100℃ / min, and the axial pressure of 30MPa is applied at the beginning of sintering; The second stage: when the sintering temperature is raised to 1300℃, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1700℃ at a heating rate of 80-100℃ / min. During this process, the Ni phase gradually forms a liquid phase as the sintering temperature increases; The third stage: when the sintering temperature is raised to 1700℃, the heating rate is reduced to 30-50℃ / min, and the temperature is gradually raised to 1800℃; The fourth stage: the heat preservation stage, heat preservation at 1800℃ for 5 minutes.

[0011] After sintering, the current is turned off and the furnace is cooled. When the temperature drops to 1300°C, the sintering pressure drops from 50MPa to 0. After the temperature continues to drop to room temperature, the sintered sample is taken out to obtain the LaB6-Ni composite material.

[0012] LaB6-4-5wt.%Ni: The first stage: the sintering temperature is increased from room temperature to 1200℃, the heating rate is 80-100℃ / min, and the axial pressure of 30MPa is applied at the beginning of sintering; The second stage: the sintering temperature is raised to 1200℃, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1400℃ at a heating rate of 80-100℃ / min; The third stage: when the sintering temperature is raised to 1400℃, the heating rate is reduced to 30-50℃ / min, and the temperature is gradually raised to 1650℃. During this process, the Ni phase gradually forms a liquid phase as the sintering temperature increases; The fourth stage: the heat preservation stage, heat preservation at 1650℃ for 5 minutes.

[0013] After sintering, the current is turned off and the furnace is cooled. When the temperature drops to 1300°C, the sintering pressure drops from 50MPa to 0. After the temperature continues to drop to room temperature, the sintered sample is taken out to obtain the LaB6-Ni composite material.

[0014] (III) Beneficial effects: The present invention provides a method for preparing a high-density LaB6-Ni composite material by spark plasma liquid phase sintering. It has the following beneficial effects: 1. In the present invention, by introducing a small amount of low-melting-point metal Ni second phase, during the spark plasma sintering process, the metal Ni forms a liquid phase as the sintering temperature increases, and then wets the LaB6 powder particles, significantly reducing the sintering temperature and sintering time, that is, a LaB6-Ni composite material is prepared by spark plasma liquid phase sintering, which has high density, high hardness, and excellent thermal electron emission performance. This method saves energy and cost and is suitable for industrial production and application of materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a physical picture of the LaB6 composite material prepared according to Example 1 of the present invention; Figure 2 A hardness comparison chart of materials prepared according to Comparative Examples 1 and 2 and Examples 1, 2 and 3 of the present invention; Figure 3 This is the corrosion morphology of the LaB6-2wt.%Ni sample; Figure 4 This is an enlarged view of the corrosion morphology of the LaB6-2wt.%Ni sample; Figure 5 This is the boron element mapping distribution map; Figure 6 This is the lanthanum element mapping distribution map; Figure 7 This is the distribution map of nickel element mapping; Figure 8 This is a comparison diagram of the volt-ampere characteristic curves of the LaB6-Ni polycrystalline composite material prepared in Example 1 and the high-density LaB6 polycrystalline prepared in Comparative Example 2 at temperatures of 1873K and 1773K. DETAILED DESCRIPTION

[0016] The present invention is described below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. Any modification and improvement made without changing the inventive concept belongs to the protection scope of the present invention.

[0017] Comparative Example 1: (1) Place the LaB6 raw material powder into a stainless steel ball mill and add stainless steel balls as the ball milling medium at a ball-to-material ratio of 10:1. Evacuate the ball mill and then fill it with argon (repeat this process 3 times) and place it in a high-energy ball mill for 8 hours at a ball milling frequency of 45 Hz.

[0018] (2) The ball-milled powder obtained in step (1) was placed in a vacuum drying oven and dried at 80°C for 12 h before being taken out.

[0019] (3) Place the dried powder into a graphite mold and wrap the powder with a thin carbon paper to isolate the graphite mold and the pressure head. Then pre-press the powder on a hydraulic press with a pre-pressure of 3MPa and place the powder in the middle of the mold. After the pre-pressing is completed, wrap a layer of carbon felt on the surface of the mold and place it in a spark plasma sintering furnace. Adjust the mold position through a graphite pad and connect the upper and lower electrodes of the sintering furnace to form a sintering current. Then evacuate to below 5Pa and start sintering. The process parameters are as follows: The first stage: the sintering temperature is increased from room temperature to 1300°C, the heating rate is 90°C / min, and an axial pressure of 30MPa is applied at the beginning of sintering; The second stage: the sintering temperature is raised to 1300°C, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1700°C at a heating rate of 90°C / min; The third stage: when the sintering temperature is raised to 1700℃, the heating rate is reduced to 30-50℃ / min, and the temperature is gradually raised to 1800℃; The fourth stage: the heat preservation stage, heat preservation at 1800℃ for 5 minutes.

[0020] After sintering is completed, the current is turned off and the furnace is cooled. When the temperature drops to 1300°C, the sintering pressure drops from 50MPa to 0. After the temperature continues to drop to room temperature, the sintered sample is taken out to obtain LaB6 polycrystal.

[0021] After testing, the density of the sample is 83.4%. Vickers hardness value is as follows Figure 2 As shown, the Vickers hardness of the sample is 7.63 GPa.

[0022] Comparative Example 2: (1) Place the LaB6 raw material powder into a stainless steel ball mill and add stainless steel balls as the ball milling medium at a ball-to-material ratio of 10:1. Evacuate the ball mill and then fill it with argon (repeat this process 3 times) and place it in a high-energy ball mill for 8 hours at a ball milling frequency of 45 Hz.

[0023] (2) The ball-milled powder obtained in step (1) was placed in a vacuum drying oven and dried at 80°C for 12 h before being taken out.

[0024] (3) Place the dried powder into a graphite mold and wrap the powder with a thin carbon paper to isolate the graphite mold and the pressure head. Then pre-press the powder on a hydraulic press with a pre-pressure of 3MPa and place the powder in the middle of the mold. After the pre-pressing is completed, wrap a layer of carbon felt on the surface of the mold and place it in a spark plasma sintering furnace. Adjust the mold position through a graphite pad and connect the upper and lower electrodes of the sintering furnace to form a sintering current. Then evacuate to below 5Pa and start sintering. The process parameters are as follows: The first stage: the sintering temperature is increased from room temperature to 1000°C, the heating rate is 60°C / min, and an axial pressure of 30MPa is applied at the beginning of sintering; The second stage: when the sintering temperature is raised to 1000℃, the heating rate is reduced to 30℃ / min, and then gradually raised to 1700℃. During this process, the sintering pressure remains unchanged. The third stage: the sintering temperature is raised to 1700℃, the sintering pressure is increased from 30MPa to 40MPa, and the temperature is continued to rise to 1900℃ at 30℃ / min; The fourth stage: the sintering temperature is raised to 1900°C, the sintering pressure is increased from 40MPa to 50MPa, and the temperature is continued to rise to 1950°C at 30°C / min; The fifth stage: the heat preservation stage, heat preservation at 1950℃ for 20 minutes.

[0025] After sintering is completed, the current is turned off and the furnace is cooled. When the temperature drops to 1200°C, the sintering pressure drops from 50MPa to 40MPa. When the temperature continues to drop to 800°C, the sintering pressure drops from 40MPa to 0. After it reaches room temperature, the sintered sample is taken out to obtain LaB6 polycrystal.

[0026] After testing, the density of the sample is 97.0%. Vickers hardness value is as follows Figure 2 As shown, the Vickers hardness of the sample is 19.4 GPa.

[0027] Embodiment 1: (1) LaB6 powder and metal Ni powder are weighed and filled into cans according to the mass fraction of Ni of 2 wt.%, and then loaded into a powder mixer for mixing to obtain uniform powder.

[0028] (2) The mixed powder obtained in step (1) was placed in a stainless steel ball mill, and stainless steel balls were added as a ball milling medium at a ball-to-material ratio of 10:1. The ball mill was evacuated and then filled with argon (this process was repeated 3 times) and then placed in a high-energy ball mill for 8 hours at a ball milling frequency of 45 Hz.

[0029] (3) The ball-milled powder obtained in step (2) was placed in a vacuum drying oven and dried at 80°C for 12 h before being taken out.

[0030] (4) Put the dried powder into the graphite mold, wrap the powder with thin carbon paper to isolate the graphite mold and the pressure head, and then pre-press the powder on the hydraulic press with a pre-pressure of 3MPa, and place the powder in the middle of the mold. After the pre-pressing is completed, wrap a layer of carbon felt on the surface of the mold and place it in the spark plasma sintering furnace. Adjust the mold position through the graphite pad and connect the upper and lower electrodes of the sintering furnace to form a sintering current. Then evacuate to below 5Pa and start sintering. The process parameters are as follows: The first stage: the sintering temperature is increased from room temperature to 1300°C, the heating rate is 80°C / min, and an axial pressure of 30MPa is applied at the beginning of sintering; The second stage: when the sintering temperature is raised to 1300℃, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1700℃ at a heating rate of 90℃ / min. During this process, the Ni phase gradually forms a liquid phase as the sintering temperature increases; The third stage: when the sintering temperature is raised to 1700℃, the heating rate is reduced to 30℃ / min and the temperature is gradually raised to 1800℃; The fourth stage: the heat preservation stage, heat preservation at 1800℃ for 5 minutes.

[0031] After sintering is completed, turn off the current and cool with the furnace. When the temperature drops to 1300℃, the sintering pressure drops from 50MPa to 0. After further cooling to room temperature, take out the sintered sample to obtain the LaB6-Ni composite material. Figure 1 shown.

[0032] After testing, the density of the sample is 97.5%, and the Vickers hardness value is Figure 2 As shown, the Vickers hardness of the sample is 21.9 GPa. Compared with the 83.4% LaB6 polycrystal obtained in Comparative Example 1, the LaB6-Ni composite material obtained in this embodiment has higher density and greater hardness. Compared with the 97.0% LaB6 polycrystal obtained in Comparative Example 2, the LaB6-Ni composite material obtained in this embodiment has a comparable density, but the sintering temperature of this embodiment is lower and the insulation time is shorter, so it saves more energy and cost, and is more suitable for the industrial production and application of materials. Compared with the LaB6 polycrystals of the same density, the LaB6-Ni composite material obtained in this embodiment has a greater hardness. Figure 3-7 It can be seen that the LaB6-Ni composite material has an obvious two-phase structure, and the Ni phase is mainly distributed between the LaB6 grains. Figure 8 It can be found from the volt-ampere characteristic curve of the thermal electron emission performance that under the same cathode operating conditions, compared with the 97.0% density LaB6 polycrystal obtained in Comparative Example 2, the thermal electron emission current density of the LaB6-Ni composite material obtained in this embodiment is higher, that is, the thermal electron emission performance of the LaB6-Ni composite material is better.

[0033] Embodiment 2: (1) LaB6 powder and metal Ni powder were weighed and filled into cans according to the Ni mass fraction of 0.7 wt.%, and then loaded into a powder mixer for mixing to obtain uniform powder.

[0034] (2) The mixed powder obtained in step (1) was placed in a stainless steel ball mill, and stainless steel balls were added as a ball milling medium at a ball-to-material ratio of 10:1. The ball mill was evacuated and then filled with argon (this process was repeated 3 times), and then placed in a high-energy ball mill for 8 hours at a ball milling frequency of 45 Hz.

[0035] (3) The ball-milled powder obtained in step (2) was placed in a vacuum drying oven and dried at 80°C for 12 h before being taken out.

[0036] (4) Place the dried powder into a graphite mold and wrap the powder with a thin carbon paper to isolate the graphite mold and the pressure head. Then pre-press the powder on a hydraulic press with a pre-pressure of 3MPa and place the powder in the middle of the mold. After the pre-pressing is completed, wrap a layer of carbon felt on the surface of the mold and place it in a spark plasma sintering furnace. Adjust the mold position through a graphite pad and connect the upper and lower electrodes of the sintering furnace to form a sintering current. Then evacuate to below 5Pa and start sintering. The process parameters are as follows: The first stage: the sintering temperature is increased from room temperature to 1300°C, the heating rate is 90°C / min, and an axial pressure of 30MPa is applied at the beginning of sintering; The second stage: when the sintering temperature is raised to 1300℃, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1700℃ at a heating rate of 90℃ / min. During this process, the Ni phase gradually forms a liquid phase as the sintering temperature increases; The third stage: when the sintering temperature is raised to 1700℃, the heating rate is reduced to 40℃ / min and the temperature is gradually raised to 1800℃; The fourth stage: the heat preservation stage, heat preservation at 1800℃ for 5 minutes.

[0037] After sintering, the current is turned off and the furnace is cooled. When the temperature drops to 1300°C, the sintering pressure drops from 50MPa to 0. After the temperature continues to drop to room temperature, the sintered sample is taken out to obtain the LaB6-Ni composite material.

[0038] After testing, the density of the sample is 94.3%, and the Vickers hardness value is Figure 2 As shown, the Vickers hardness of the sample is 18.5 GPa. Compared with the 83.4% LaB6 polycrystal obtained in Comparative Example 1, the LaB6-Ni composite material obtained in this example has higher density and greater hardness.

[0039] Embodiment 3: (1) LaB6 powder and metal Ni powder are weighed and filled into cans according to the mass fraction of Ni of 5 wt.%, and then loaded into a powder mixer for mixing to obtain uniform powder.

[0040] (2) The mixed powder obtained in step (1) was placed in a stainless steel ball mill, and stainless steel balls were added as a ball milling medium at a ball-to-material ratio of 10:1. The ball mill was evacuated and then filled with argon (this process was repeated 3 times), and then placed in a high-energy ball mill for 8 hours at a ball milling frequency of 45 Hz.

[0041] (3) The ball-milled powder obtained in step (2) was placed in a vacuum drying oven and dried at 80°C for 12 h before being taken out.

[0042] (4) Place the dried powder into a graphite mold and wrap the powder with a thin carbon paper to isolate the graphite mold and the pressure head. Then pre-press the powder on a hydraulic press with a pre-pressure of 3MPa and place the powder in the middle of the mold. After the pre-pressing is completed, wrap a layer of carbon felt on the surface of the mold and place it in a spark plasma sintering furnace. Adjust the mold position through a graphite pad and connect the upper and lower electrodes of the sintering furnace to form a sintering current. Then evacuate to below 5Pa and start sintering. The process parameters are as follows: The first stage: the sintering temperature is increased from room temperature to 1200°C, the heating rate is 100°C / min, and an axial pressure of 30MPa is applied at the beginning of sintering; The second stage: the sintering temperature is raised to 1200°C, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1400°C at a heating rate of 90°C / min; The third stage: when the sintering temperature is raised to 1400℃, the heating rate is reduced to 50℃ / min and the temperature is gradually raised to 1650℃. During this process, the Ni phase gradually forms a liquid phase as the sintering temperature increases. The fourth stage: the heat preservation stage, heat preservation at 1650℃ for 5 minutes.

[0043] After sintering, the current is turned off and the furnace is cooled. When the temperature drops to 1300°C, the sintering pressure drops from 50MPa to 0. After the temperature continues to drop to room temperature, the sintered sample is taken out to obtain the LaB6-Ni composite material.

[0044] After testing, the density of the sample is 99.2%, and the Vickers hardness value is Figure 2 As shown, the Vickers hardness of the sample is 23.8 GPa. Compared with the 83.4% LaB6 polycrystal obtained in Comparative Example 1 and the 97.0% LaB6 polycrystal obtained in Comparative Example 2, the LaB6-Ni composite material obtained in this example has higher density and greater hardness.

[0045] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention. Finally, it should be noted that the foregoing are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it will be still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention shall be included in the scope of the present invention as defined by the appended claims and their equivalents.

Claims

1. A method for preparing a high-density LaB6-Ni composite material by spark plasma liquid phase sintering, characterized in that: The method comprises weighing and canning LaB6 powder and metal Ni powder in different proportions, wherein the mass fraction of Ni is 0wt.%-5wt.%, and then loading the powder into a powder mixer for mixing to obtain uniform powder, comprising the following steps: Step (1) placing the obtained mixed powder into a stainless steel ball mill, adding stainless steel balls as a ball milling medium at a ball-to-material ratio of 10:1, evacuating the ball mill and then filling it with argon, repeating this process three times, placing the mixed powder into a high-energy ball mill, and milling for 8 hours at a ball milling frequency of 45 Hz; Step (2) placing the ball-milled powder obtained in step (1) into a vacuum drying oven, drying at 80° C. for 12 h, and then taking it out; Step (3) loading the dried powder into a graphite mold, wrapping the powder with a thin carbon paper to isolate the graphite mold and the pressing head, and then pre-pressing the powder on a hydraulic press with a pre-pressure of 3 MPa, and placing the powder in the middle of the mold; Step (4) placing the pre-pressed powder in a spark plasma sintering furnace, adjusting the mold position by means of a graphite pad and connecting the upper and lower electrodes of the sintering furnace so that a sintering current can be generated; Step (5) evacuating the vacuum to below 5 Pa and starting the reaction sintering; Step (6) After sintering is completed, the current is turned off and the furnace is cooled. When the temperature drops to 1300°C, the sintering pressure drops from 50 MPa to 0. After the temperature continues to drop to room temperature, the sintered sample is taken out.

2. The method according to claim 1, characterized in that Sintering process of LaB6-Ni composite material formed by doping LaB6-0-4wt.%Ni: The first stage: the sintering temperature is increased from room temperature to 1300℃, the heating rate is 80-100℃ / min, and the axial pressure of 30MPa is applied at the beginning of sintering; The second stage: when the sintering temperature is raised to 1300℃, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1700℃ at a heating rate of 80-100℃ / min. During this process, the Ni phase gradually forms a liquid phase as the sintering temperature increases; The third stage: when the sintering temperature is raised to 1700℃, the heating rate is reduced to 30-50℃ / min, and the temperature is gradually raised to 1800℃; The fourth stage: the heat preservation stage, heat preservation at 1800℃ for 5 minutes; After sintering, the current was turned off and the furnace was cooled. When the temperature dropped to 1300°C, the sintering pressure dropped from 50MPa to 0. After the temperature continued to drop to room temperature, the sintered sample was taken out to obtain the LaB6-Ni composite material.

3. The method according to claim 2, characterized in that Sintering process of LaB6-Ni composite material formed by doping LaB6-4-5wt.%Ni: The first stage: the sintering temperature is increased from room temperature to 1200℃, the heating rate is 80-100℃ / min, and the axial pressure of 30MPa is applied at the beginning of sintering; The second stage: the sintering temperature is raised to 1200℃, the sintering pressure is increased from 30MPa to 50MPa, and the temperature is continued to rise to 1400℃ at a heating rate of 80-100℃ / min; The third stage: when the sintering temperature is raised to 1400℃, the heating rate is reduced to 30-50℃ / min, and the temperature is gradually raised to 1650℃. During this process, the Ni phase gradually forms a liquid phase as the sintering temperature increases; The fourth stage: heat preservation stage, heat preservation at 1650℃ for 5 minutes; After sintering, the current was turned off and the furnace was cooled. When the temperature dropped to 1300°C, the sintering pressure dropped from 50MPa to 0. After the temperature continued to drop to room temperature, the sintered sample was taken out to obtain the LaB6-Ni composite material.

Citation Information

Patent Citations

  • Lanthanum-calcium composite hexaboride polycrystalline cathode material and preparation method thereof

    CN112723891A

  • Boride ceramics for electrode, electrode obtained by using the same, and method of producing boride ceramics for electrode

    JP2004250725A

Cited By

  • Polycrystal lanthanum hexaboride and preparation method and application thereof

    CN120136556A

  • Polycrystalline lanthanum hexaboride, and preparation method and application thereof

    CN120136556B

  • Hard alloy bar vacuum sintering process capable of preventing deformation

    CN120885685A