High-conductivity wear-resistant copper-based composite material and preparation process thereof

Through special oxidation and addition processes and hot forging and cold rolling deformation, uniformly distributed copper oxide particles are formed, which solves the contradiction between wear resistance and conductive properties of copper-based composite materials, and realizes the preparation of copper-based composite materials with high conductivity and wear resistance. in mass production.

CN118910456APending Publication Date: 2024-11-08MCC KUNYUAN (CHONGQING) METAL MATERIALS RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997084.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When existing copper-based composite materials improve wear resistance, they are prone to damage their conductivity, and traditional powder metallurgy processes have problems such as difficult preparation, small sample size and high cost, which limits their large-scale production.

Method used

Using special oxidation and addition processes, through step temperature oxidation and molten salt, uniformly distributed copper oxide particles are formed, combined with hot forging and cold rolling deformation, significantly improving the wear resistance of copper-based composite materials while maintaining high conductivity. .

Benefits of technology

The preparation of high-conductive wear-resistant copper-based composite materials is realized. The copper oxide particles play a lubricating role in the friction process, significantly reducing the friction coefficient and wear amount, improving the wear resistance of the material, and avoiding copper oxide caused by density difference. Upload problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910456A_ABST
    Figure CN118910456A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of copper-based composite material preparation, and relates to a high-conductivity wear-resistant copper-based composite material and a preparation process thereof.The preparation process comprises the following steps that high-purity spherical copper powder and fused salt are weighed according to a certain volume ratio and mixed, and mixed powder is obtained; the mixed powder is placed in a heating container and placed in a heating furnace, air is introduced for heating oxidation, the oxidation temperature changes in a stepped mode, the mixed powder is cooled along with the furnace after heating oxidation, and pretreated mixed powder is obtained; melting copper or copper alloy to obtain a melt, briquetting the pretreated mixed powder, adding the melt, uniformly stirring, and casting after stirring to obtain a cast ingot; and the cast ingot is taken out and subjected to hot forging, hot rolling and cold rolling are sequentially conducted after hot forging, and the high-conductivity wear-resisting copper-based composite material is obtained. According to the high-conductivity wear-resistant copper-based composite material, a large number of micron-sized copper oxide particles are uniformly distributed in a matrix, so that the friction coefficient and the abrasion loss of the high-conductivity wear-resistant copper-based composite material are effectively reduced, and the conductivity is maintained while the wear resistance is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper-based composite material preparation, and relates to a highly conductive and wear-resistant copper-based composite material and a preparation process thereof. Background Art

[0002] With the development of industrial technology, complex service environments have increasingly stringent requirements for copper-based composite materials. Pure copper, as the most widely used conductive material in industry, has the advantages of high conductivity and easy forming. However, due to its low strength and poor wear resistance, some application scenarios that require high conductivity and high wear resistance cannot meet the requirements. At present, the demand for copper-based composite materials in many industrial fields has evolved from high strength and high conductivity to high conductivity and wear resistance. While ensuring excellent conductivity, it also has higher wear resistance, which poses new challenges to copper alloys and copper-based composite materials.

[0003] In the preparation of copper-based composite materials, it is usually necessary to introduce second phase particles for organization and performance regulation. However, many hard second phases (such as borides, carbides, oxides, etc.) added to the pure copper matrix may cause adverse factors to the conductivity while improving the wear resistance. In addition, it will cause processing difficulties and cannot be industrialized on a large scale. Copper oxide is a common copper oxide, which is usually added to the copper matrix using processes such as powder metallurgy. It plays a lubricating role during the friction process, reduces the friction coefficient, and reduces the amount of wear. However, the traditional powder metallurgy process has disadvantages such as difficult preparation, small sample size, and high cost, which limit its large-scale production. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a highly conductive and wear-resistant copper-based composite material and a preparation process thereof, which, through a special oxidation and addition process, significantly improves the wear resistance of the copper-based composite material while maintaining the high conductivity and high ductility of the pure copper matrix.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A preparation process of a highly conductive and wear-resistant copper-based composite material comprises the following steps:

[0007] S1. Mixed powder:

[0008] Weighing a certain volume ratio of high-purity spherical copper powder and molten salt and mixing them to obtain mixed powder;

[0009] S2. Step temperature oxidation:

[0010] The mixed powder is placed in a heating container and placed in a heating furnace, air is introduced for heating and oxidation, and the oxidation temperature is stepwise changed, and after heating and oxidation, the mixed powder is cooled with the furnace to obtain a pre-treated mixed powder;

[0011] S3. Melting and compounding:

[0012] The copper or copper alloy is melted to obtain a melt, the pre-treated mixed powder is pressed into blocks, added to the melt and stirred evenly, and after the stirring is completed, casting is performed to obtain an ingot;

[0013] S4. Post-deformation processing:

[0014] The ingot is taken out and hot forged, and then hot rolled and cold rolled in sequence to obtain a highly conductive and wear-resistant copper-based composite material.

[0015] Furthermore, the heating container is a corundum boat, and the heating furnace is a tubular furnace.

[0016] Furthermore, in step S1, a mixer is used for mixing, and the rotation speed is controlled to be 100-350 r / min, and the mixing time is 5-30 min.

[0017] Furthermore, in step S1, the volume ratio of the high-purity spherical copper powder to the molten salt is in the range of 1:5-1:30.

[0018] Furthermore, in step S1, the particle size of the high-purity spherical copper powder is 0.1-100 μm.

[0019] Furthermore, the molten salt includes one or more of chloride, fluoride and boride, which mainly acts as a carrier and breaks up the copper oxide film.

[0020] Furthermore, in step S2, the air flow rate is 0.5L / min-120L / min, and the maximum oxidation temperature does not exceed the melting point of the salt. Preferably, the maximum oxidation temperature is in the range of 0.6-0.9T. 盐 .

[0021] Furthermore, in step S2, the stepwise change of the oxidation temperature includes:

[0022] 100℃-200℃, keep warm evenly for 0.5-12h. The purpose of this stage is to fully release the stress generated during the preparation of spherical powder;

[0023] 200-400℃, uniformly keep warm for 0.5-12h. The purpose of this stage is to achieve rapid oxidation of copper powder and gradually thicken the oxide film layer;

[0024] 400℃-600℃, uniform heat preservation for 0 / 5-12h. The purpose of this stage is to achieve partial bonding of salt and oxide film through the reaction between salt and oxide film.

[0025] Further, in step S3, a medium frequency induction furnace is used to melt copper or copper alloy, and the smelting temperature is 900℃-1450℃; the stirring method is mechanical stirring, the stirring speed is 50rpm-450rpm, the stirring time is 5-30min, and a water-cooled mold is used for casting. In this process, the powder block pressed by the pre-treated mixed powder is rapidly melted in the melt, the molten salt dissolves part of the copper oxide film, and the copper powder melts inside, and the two act to break most of the copper oxide particles and disperse them in the molten salt; the density of the copper oxide particles is between the molten salt melt and the copper melt, so the copper oxide is first dispersed at the interface between the molten salt and the copper, and diffuses to the copper melt under the action of mechanical stirring; the molten salt can also isolate oxygen in the air to prevent the melt from being violently oxidized.

[0026] Furthermore, in step S4, the hot rolling deformation amount is 10%-50%, and the cold rolling deformation amount is 10%-90%.

[0027] A highly conductive and wear-resistant copper-based composite material, comprising a highly conductive and wear-resistant copper-based composite material prepared by the above-mentioned preparation process of the highly conductive and wear-resistant copper-based composite material, wherein the matrix of the highly conductive and wear-resistant copper-based composite material is highly conductive pure copper or copper alloy, and CuO particles are uniformly distributed at grain boundaries and in grains;

[0028] The alloy elements of the copper alloy include Ag, Cd, Cr and Zr, and the size of CuO particles is 0.01-500 μm.

[0029] The beneficial effects of the present invention are:

[0030] The present invention provides a highly conductive and wear-resistant copper-based composite material and a preparation process thereof. Based on a highly conductive pure copper and copper alloy matrix, a special oxidation process is used to form an oxide film on high-purity spherical copper powder. The oxide film can be evenly mixed with the melt under the action of molten salt, thereby avoiding the problem of floating due to density difference after adding copper oxide in the traditional process. At the same time, the preparation process accurately controls the smelting temperature so that the melt viscosity is within a suitable range, significantly reducing the floating of copper oxide caused by density difference. Subsequently, hot forging, hot rolling and cold rolling deformation are performed to further achieve uniform distribution of copper oxide in the matrix, while introducing a large number of dislocations inside the plate to improve the final use performance of the material.

[0031] The present invention ultimately obtains a highly conductive and wear-resistant copper-based composite material in which a large number of micron-sized copper oxide particles are uniformly distributed inside the matrix. The copper oxide particles play a lubricating role during the friction process, effectively reducing the friction coefficient and wear amount of the highly conductive and wear-resistant copper-based composite material, thereby significantly improving the wear resistance while maintaining the conductivity.

[0032] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0034] Figure 1 is a SEM image of the copper oxide reinforced copper-based composite material in Example 1;

[0035] Figure 2 is the EDS image of the copper oxide reinforced copper-based composite material in Example 1;

[0036] Figure 3 This is the SEM image of the copper oxide reinforced copper-based composite material in Comparative Example 2. DETAILED DESCRIPTION

[0037] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.

[0038] Among them, the drawings are only used for illustrative explanations, and they only represent schematic diagrams rather than actual pictures, and should not be understood as limitations on the present invention. In order to better illustrate the embodiments of the present invention, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of actual products. For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted.

[0039] The same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right", "front", "rear", etc. indicate the orientation or position relationship, they are based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the terms describing the position relationship in the drawings are only used for illustrative purposes and cannot be understood as limiting the present invention. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.

[0040] Example 1

[0041] A high-conductivity, wear-resistant copper-based composite material, the preparation method of which comprises the following steps:

[0042] 1) Mixed powder:

[0043] Weigh high-purity spherical copper powder and potassium fluoroaluminate in a volume ratio of 1:20, and mix them in a mixer at a speed of 200 r / min for 10 min;

[0044] The particle size of the high-purity spherical copper powder is 18-53 microns;

[0045] 2) Step temperature oxidation:

[0046] The mixed powder was placed in a corundum boat, placed in a tubular furnace, and air was introduced for oxidation. The air flow rate was 10 L / min, and the oxidation temperature was changed in steps: 150°C, uniformly kept warm for 0.5 h; 300°C, uniformly kept warm for 1 h; 550°C, uniformly kept warm for 2 h, and then cooled with the furnace;

[0047] 3) Melting compound:

[0048] Use a medium frequency induction furnace to melt copper or copper alloy at a melting temperature of 1150°C;

[0049] The powder prepared in 2) was pressed into a block and added into the melt, and mechanically stirred for 20 min at a speed of 150 rpm;

[0050] After the mixing is completed, the casting is carried out using a water-cooled mold;

[0051] 4) Post-deformation processing

[0052] After the ingot is taken out, it is hot forged, forged to a suitable shape and then hot rolled, with a hot rolling deformation of 50%;

[0053] The material is cold rolled to a suitable thickness with a cold rolling deformation of 70% to obtain a high-conductivity and wear-resistant copper-based composite material.

[0054] Specifically, the pre-treated mixed powder is briquetting by a briquetting process commonly used in the prior art, and the purpose of briquetting can be achieved. In this embodiment, the following process parameters are adopted: the pressing pressure of the briquetting is 20-600Mpa, and the pressure holding time is 5-30s.

[0055] like Figure 1 and Figure 2 As shown, the high-conductivity and wear-resistant copper-based composite material prepared in this embodiment was cut into pieces for testing, and the conductivity and friction performance are shown in Table 1. A scanning electron microscope sample was prepared for observation and morphology analysis and energy spectrum analysis were performed, as shown in FIG. Figure 1 and Figure 2 shown.

[0056] Table 1 EDS intelligent quantitative results

[0057]

[0058] The SEM and EDS characterization results showed that a large number of micron-sized CuO particles were evenly distributed in the pure copper matrix. EDS energy spectrum analysis found that trace Al elements (derived from potassium fluoroaluminate molten salt) were detected in some CuO particles, indicating that the molten salt reacted with the oxide film during the composite process, further indicating that the molten salt promoted the entry of copper oxide particles into the copper matrix.

[0059] Example 2

[0060] A high-conductivity, wear-resistant copper-based composite material, the preparation method of which comprises the following steps:

[0061] 1) Mixed powder:

[0062] Weigh high-purity spherical copper powder and salt (sodium chloride and potassium fluoroaluminate mixed in a ratio of 1:15 by volume) and mix them in a mixer at a speed of 220 r / min for 20 min.

[0063] The particle size of the high-purity spherical copper powder is 18-53 microns;

[0064] 2) Step temperature oxidation:

[0065] The mixed powder was placed in a corundum boat, placed in a tubular furnace, and air was introduced for oxidation. The air flow rate was 20 L / min, and the oxidation temperature was changed in steps: 150°C, uniformly kept warm for 0.5 h; 350°C, uniformly kept warm for 1 h; 500°C, uniformly kept warm for 3 h, and then cooled with the furnace;

[0066] 3) Melting compound:

[0067] Use a medium frequency induction furnace to melt copper or copper alloy at a melting temperature of 1250°C;

[0068] The powder prepared in 2) was pressed into a block and added into the melt, and mechanically stirred for 30 min at a speed of 250 rpm;

[0069] After the mixing is completed, the casting is carried out using a water-cooled mold;

[0070] 4) Post-deformation processing

[0071] After the ingot is taken out, it is hot forged, forged to a suitable shape and then hot rolled, with a hot rolling deformation of 50%;

[0072] The material is cold rolled to a suitable thickness with a cold rolling deformation of 70% to obtain a high-conductivity and wear-resistant copper-based composite material.

[0073] Example 3

[0074] A high-conductivity, wear-resistant copper-based composite material, the preparation method of which comprises the following steps:

[0075] 1) Mixed powder:

[0076] Weigh high-purity spherical pure powder and potassium fluoroaluminate in a volume ratio of 1:25, and mix them using a mixer at a speed of 220 r / min and a mixing time of 20 min;

[0077] The particle size of the high-purity spherical copper powder is 18-53 microns;

[0078] 2) Step temperature oxidation:

[0079] The mixed powder was placed in a corundum boat, placed in a tubular furnace, and air was introduced for oxidation. The air flow rate was 30 L / min, and the oxidation temperature was changed in steps: 120°C, uniformly kept warm for 0.5 h; 320°C, uniformly kept warm for 1 h; 550°C, uniformly kept warm for 3 h, and then cooled with the furnace;

[0080] 3) Melting compound:

[0081] The Cu-2Ag alloy was melted using a medium frequency induction furnace at a melting temperature of 1200°C;

[0082] The powder prepared in 2) was pressed into a block and added into the melt, and mechanically stirred for 40 min at a speed of 300 rpm;

[0083] After the mixing is completed, the casting is carried out using a water-cooled mold;

[0084] 4) Post-deformation processing

[0085] After the ingot is taken out, it is hot forged, forged to a suitable shape and then hot rolled, with a hot rolling deformation of 50%;

[0086] The material is cold rolled to a suitable thickness with a cold rolling deformation of 70% to obtain a high-conductivity and wear-resistant copper-based composite material.

[0087] Comparative Example 1 (Compared with Example 1, high-purity copper oxide powder was directly added)

[0088] A high-conductivity, wear-resistant copper-based composite material, the preparation method of which comprises the following steps:

[0089] 1) Mixed powder:

[0090] Weigh high-purity copper oxide powder and potassium fluoroaluminate in a volume ratio of 1:20, and mix them using a mixer at a speed of 200 r / min for 10 min;

[0091] The particle size of the high-purity spherical copper oxide powder is 18-53 microns;

[0092] 2) Step temperature oxidation:

[0093] The mixed powder was placed in a corundum boat, placed in a tubular furnace, and air was introduced for oxidation. The air flow rate was 10 L / min, and the oxidation temperature was changed in steps: 150°C, uniformly kept warm for 0.5 h; 300°C, uniformly kept warm for 1 h; 550°C, uniformly kept warm for 2 h, and then cooled with the furnace;

[0094] 3) Melting compound:

[0095] Use a medium frequency induction furnace to melt copper or copper alloy at a melting temperature of 1150°C;

[0096] The powder prepared in 2) was pressed into a block and added into the melt, and mechanically stirred for 20 min at a speed of 150 rpm;

[0097] After the mixing is completed, the casting is carried out using a water-cooled mold;

[0098] 4) Post-deformation processing:

[0099] After the ingot is taken out, it is hot forged, forged to a suitable shape and then hot rolled, with a hot rolling deformation of 50%;

[0100] The material is cold rolled to a suitable thickness with a cold rolling deformation of 70% to obtain a high-conductivity and wear-resistant copper-based composite material.

[0101] The high-conductivity, wear-resistant copper-based composite material prepared in this embodiment was cut into pieces for testing. The conductivity and friction properties are shown in Table 2. No copper oxide was found by scanning electron microscopy, indicating that the copper oxide powder floated up to form slag due to density difference during the smelting stage and was not successfully added to the matrix.

[0102] Comparative Example 2 (Compared with Example 1, step temperature oxidation was not used)

[0103] A high-conductivity, wear-resistant copper-based composite material, the preparation method of which comprises the following steps:

[0104] 1) Mixed powder:

[0105] Weigh high-purity spherical copper powder and potassium fluoroaluminate in a volume ratio of 1:20, and mix them in a mixer at a speed of 200 r / min for 10 min;

[0106] The particle size of the high-purity spherical copper powder is 18-53 microns.

[0107] 2) Oxidation:

[0108] The mixed powder was placed in a corundum boat, placed in a tubular furnace, and air was introduced for oxidation at an air flow rate of 10 L / min. The temperature was maintained at 550°C and the mixture was evenly kept warm for 2 hours before being cooled with the furnace.

[0109] 3) Melting compound:

[0110] Use a medium frequency induction furnace to melt copper or copper alloy at a melting temperature of 1150°C;

[0111] The powder prepared in 2) was pressed into a block and added into the melt, and mechanically stirred for 20 min at a speed of 150 rpm;

[0112] After stirring, casting is carried out using a water-cooled mold.

[0113] 4) Post-deformation processing:

[0114] After the ingot is taken out, it is hot forged, forged to a suitable shape and then hot rolled, with a hot rolling deformation of 50%;

[0115] Cold rolled to appropriate thickness, with cold rolling deformation of 70%.

[0116] The ingot prepared in this comparative example was cut into pieces to prepare scanning electron microscope samples for observation and energy spectrum analysis. Figure 3 As shown, it can be seen that compared with Example 1, although the copper oxide reinforcement is partially incorporated in Comparative Example 2, the particle size is small and the dispersion is uneven. It is mainly enriched at the grain boundaries, which will affect the strength and ductility of the material.

[0117] The ingots prepared in the above examples and comparative examples were cut into pieces for testing. The electrical conductivity and friction performance are shown in Table 2:

[0118] Table 2 Performance test results

[0119]

[0120] The results in Table 2 show that, compared with the 100% IACS conductivity of pure copper, after adding copper oxide reinforcement, the conductivity of the composite material is still at a high level. With the addition of copper oxide reinforcement, it will play the role of lubricant in the friction process, so the friction coefficient can be significantly reduced. As shown in Example 1, compared with Comparative Example 1, the friction coefficient is reduced from 0.86 of pure copper to 0.45, and the wear volume is reduced from 0.2104 mm3 to 0.0789 mm3, and the wear resistance is significantly improved. Compared with Example 1, Example 2 uses different parameters of the same process, and the conductivity, friction The friction coefficient and wear volume are slightly lower than those of Example 1, but are still significantly higher than those of Comparative Examples 1 and 2. In Comparative Example 1, due to the direct addition of copper oxide powder, it has been observed that the copper oxide powder floats on the surface of the melt during smelting and does not enter the matrix. The subsequent scanning electron microscope observation also did not find that the copper oxide powder enters the matrix, indicating that the powder mixing process has an important influence on the patent of the present invention. The difference between Example 1 and Comparative Example 2 is that step temperature oxidation is not used. Although copper oxide is able to enter the matrix in Comparative Example 2, its distribution state, conductivity, and wear resistance performance indicators are all lower than those of Example 1, indicating that the step temperature oxidation process also has an important influence on the present invention.

[0121] The present invention forms an oxide film on the spherical copper powder through a special oxidation process. The oxide film can be evenly mixed with the melt under the action of salt, thereby avoiding the floating of copper oxide due to density difference after the addition of copper oxide in the traditional process. At the same time, the present process can accurately control the smelting temperature so that the melt viscosity is within a suitable range, significantly reducing the floating of copper oxide caused by density difference, and then through hot forging, hot rolling and cold rolling deformation, further achieving uniform distribution of copper oxide in the matrix, while introducing a large number of dislocations inside the plate, thereby improving the final use performance of the material.

[0122] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A preparation process of a highly conductive and wear-resistant copper-based composite material, characterized in that: The following steps are involved: S1. Mixed powder: Weighing a certain volume ratio of spherical pure copper powder and molten salt and mixing them to obtain mixed powder; S2. Step temperature oxidation: The mixed powder is placed in a heating container and placed in a heating furnace, air is introduced for heating and oxidation, and the oxidation temperature is stepwise changed, and after heating and oxidation, the mixed powder is cooled with the furnace to obtain a pre-treated mixed powder; S3. Melting and compounding: The copper or copper alloy is melted to obtain a melt, the pre-treated mixed powder is pressed into blocks, added to the melt and stirred evenly, and after the stirring is completed, casting is performed to obtain an ingot; S4. Post-deformation processing: The ingot is taken out and hot forged, and then hot rolled and cold rolled in sequence to obtain a highly conductive and wear-resistant copper-based composite material.

2. The preparation process of the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: In step S1, a mixer is used for mixing, and the rotation speed is controlled to be 100-350 r / min, and the mixing time is 5-30 min.

3. The preparation process of the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: In step S1, the volume ratio of the high-purity spherical copper powder to the molten salt is in the range of 1:5-1:

30.

4. The process for preparing the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: In step S1, the particle size of the high-purity spherical copper powder is 0.1-100 μm.

5. The preparation process of the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: The molten salt includes one or more of chloride, fluoride and boride.

6. The process for preparing the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: In step S2, the air flow rate is 0.5L / min-120L / min, and the maximum oxidation temperature ranges from 0.6T to 0.9T. 盐 .

7. The process for preparing the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: In step S2, the step change of the oxidation temperature includes: 100℃-200℃, uniform heat preservation for 0.5-12h; 200-400℃, uniform heat preservation for 0.5-12h; 400℃-600℃, uniform heat preservation 0 / 5-12h.

8. The process for preparing the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: In step S3, a medium frequency induction furnace is used to melt copper or copper alloy at a melting temperature of 900°C-1450°C; the stirring method is mechanical stirring, the stirring speed is 50rpm-450rpm, the stirring time is 5-30min, and a water-cooled mold is used for casting.

9. The process for preparing the highly conductive and wear-resistant copper-based composite material according to claim 1, characterized in that: In step S4, the hot rolling deformation amount is 10%-50%, and the cold rolling deformation amount is 10%-90%.

10. A highly conductive and wear-resistant copper-based composite material, characterized in that: A highly conductive and wear-resistant copper-based composite material prepared by the preparation process of the highly conductive and wear-resistant copper-based composite material according to any one of claims 1 to 9, wherein the matrix of the highly conductive and wear-resistant copper-based composite material is highly conductive pure copper or copper alloy, and CuO particles are uniformly distributed at grain boundaries and in grains; The alloy elements of the copper alloy include Ag, Cd, Cr and Zr, and the size of CuO particles is 0.01-500 μm.