High-cleanliness IF steel production process

Through the RH+VD dual control process, combined with the top slag modification agent and bottom bleed hydrogen deoxygenation, the problems of water outlet blockage, high alkalinity slag erosion and hydrogen-oxygen coexistence in IF steel production are solved, and the production of high-cleanness IF steel is achieved. , improving the cleanliness and alloy yield of the liquid steel.

CN118910489AActive Publication Date: 2024-11-08UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202410997277.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

There are problems such as water outlet blockage, high alkaline slag corrosion, degradation of rolled material quality and safety hazards in the existing IF steel production process, and it is difficult to effectively control the cleanliness and oxygen content of the steel liquid.

Method used

Using the RH+VD dual-control process, the liquid steel decarbonization process is carried out through RH and the top slag modification agent is added, and the bottom blown hydrogen deoxygenation and alloying is sent to the VD furnace for bottom blown hydrogen deoxygenation and alloying to avoid the use of deoxygenation alloys, and the bottom blown reducing gas is used for bottom blown Deoxygenation and remove residual hydrogen and nitrogen through the degassing capacity of VD.

Benefits of technology

It improves the cleanliness of the molten steel, reduces oxygen content, reduces safety hazards, improves the alloy yield, and achieves the production of high-cleanness IF steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of ferrous metallurgy, and particularly relates to a high-cleanliness IF steel production process, which comprises the following steps: carrying out RH + VD duplex control, carrying out molten steel decarburization treatment by adopting RH, adding a top slag modifier after RH vacuum breaking, feeding into a VD furnace, and carrying out bottom blowing hydrogen deoxidation and alloying without using a deoxidized alloy in the process. According to the method, decarburization and deoxidation are separated, potential safety hazards caused by hydrogen and oxygen coexistence are avoided, efficient top slag pre-deoxidation can be carried out through the higher molten pool stirring capacity, meanwhile, deoxidation is carried out through bottom blowing of reducing gas, the oxygen content is reduced, the risk that molten steel is secondarily oxidized by slag is avoided, and the service life of the molten steel is prolonged. And meanwhile, residual hydrogen and nitrogen are removed through the degassing capacity of VD, potential safety hazards can be reduced, the cleanliness of the molten steel can be improved, the alloy yield is increased, and production of the high-cleanliness IF steel is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a production process of high-cleanliness IF steel. Background Art

[0002] IF steel (i.e. interstitial-free steel) is widely used in the fields of automobiles, home appliances, etc. Relevant studies have shown that lightweighting of automobiles helps to reduce carbon emissions. Every 100kg reduction in automobile mass is conducive to reducing carbon dioxide emissions by 12.5g / km. At the same time, the requirements for the control of non-metallic inclusions in steel are gradually increasing due to the lightweighting of automobiles. At present, the commonly used process for producing IF steel at home and abroad is BOF / EAF-RH-CC. After RH (oxygen blowing) decarburization treatment, deoxidation and alloying operations are carried out. The main deoxidation method currently used is aluminum deoxidation, and the main deoxidation products are Al2O3 inclusions and composite inclusions formed by their combination with Ti nitrides. And the inclusions are removed by making slag with high basicity, good fluidity and low oxidation. The production process is relatively mature, but there are still some problems that cannot be avoided under the existing technology:

[0003] (1) Nozzle blockage: Al2O3 may cause problems such as continuous casting immersion nozzle nodules and nozzle blockage during the production of molten steel. Due to different requirements for rolled materials, some IF steel production cannot be treated with calcium to modify aluminum oxide inclusions. At present, scholars have proposed clean deoxidation based on carbon-oxygen reaction. Due to the extremely high requirements for carbon content of this steel, the excess oxygen after the RH stage decarburization cannot be efficiently removed in this way;

[0004] (2) High-basicity slag erosion: High-basicity slag used to remove alumina inclusions may have poor fluidity and cause serious erosion to the furnace lining and refractory materials. High-basicity slag has a high melting point, which increases the consumption of heat transfer and may cause serious slag rolling and large-sized inclusions, affecting the quality of the ingot.

[0005] (3) Rolled material quality: The Young's modulus of hard and brittle Al2O3 is larger than that of steel, which has a greater impact on the quality of rolled materials and reduces the product yield. In addition, alumina inclusions may cause local stress concentration in the material, reduce the toughness and ductility of the steel, and may also become the initiation point of fatigue cracks, reducing the fatigue life of the steel.

[0006] In order to solve the above problems, some scholars have proposed a method of pre-deoxidation by injecting reducing gas H2 after RH decarburization, but this method still has some problems:

[0007] (1) After RH oxygen blowing decarburization, composite hydrogen blowing is used. Under certain conditions, hydrogen and oxygen may coexist. When the oxygen concentration is higher than 4%, there is a safety hazard of explosion.

[0008] (2) The high oxidizability of the RH top slag may cause the later slag to transfer oxygen to the steel, resulting in secondary oxidation of the molten steel, which is not conducive to the control of the oxygen content of the molten steel. The kinetic conditions of the top slag modification after RH decarburization are poor. Summary of the invention

[0009] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a high-cleanliness IF steel production process.

[0010] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0011] A high-cleanliness IF steel production process uses RH+VD dual control to decarburize molten steel, adds top slag modifier after RH is broken, and sends it into a VD furnace for bottom-blowing hydrogen deoxidation and alloying, and no deoxidizing alloy is used in the process.

[0012] As a preferred solution of the high-cleanliness IF steel production process described in the present invention, the production process specifically includes: KR pretreatment, converter smelting, RH, VD, and continuous casting.

[0013] As a preferred solution of the high cleanliness IF steel production process described in the present invention, wherein: KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be ≤40×10 -6 .

[0014] As a preferred solution of the high-cleanliness IF steel production process described in the present invention, the following aspects are provided: the scrap steel ratio in the converter is controlled to be ≤20%; the FeO content in the slag is maintained to be ≥15wt% in the middle stage of blowing, and the FeO content in the slag is maintained to be ≤20wt% in the final stage of blowing; the converter terminal temperature is controlled to be 1690-1710°C, and the terminal [C] content is controlled to be (300-450)×10 -6 , end point [P] content ≤ 100 × 10 -6 , end point [S] content ≤ 50 × 10 -6 , end point [O] content ≥500×10 -6 ; Steel is tapped using a carbon-free ladle; 1-3 kg / t of steel is added 钢 of lime.

[0015] As a preferred solution of the high-cleanliness IF steel production process described in the present invention, the ladle car is driven to the RH station, the riser and downcomer of the RH vacuum device are immersed in the molten steel, and vacuuming is started to start the circulation; a five-stage vacuum pump is used to vacuum to 40-60 kPa and maintain it for 3-5 minutes, and a four-stage pump is started to vacuum to 5-15 kPa to maintain the vacuum degree; the lower oxygen lance starts forced decarburization, and the oxygen supply intensity is 1200-4500 NL / t 钢 / min, oxygen blowing time is 8-15min; start the third-stage pump, second-stage pump, and first-stage pump in sequence, each stage pump is maintained for 1min after being turned on, and after the last stage pump is turned on, the vacuum degree of the vacuum chamber is ≤67Pa, and the vacuum degree is maintained for 6-12min for natural decarbonization; break the air and exit the station, and the exit requirement is [C] content ≤12×10 -6 , the molten steel temperature is required to be 1665~1690℃.

[0016] As a preferred solution of the high cleanliness IF steel production process described in the present invention, 0.4-1.5 kg / t RH is added after leaving the station. 钢 The aluminum-containing top slag modifier is used, the top slag basicity is controlled at 1-2, and FeO+MnO is controlled at ≤10wt%; and it is sent to the VD station. Preferably, the aluminum-containing top slag modifier includes, by mass percentage: Al: 40%-50%, CaO: 5%-10%, Al2O3: 40%-55%.

[0017] As a preferred solution of the high-cleanliness IF steel production process described in the present invention, wherein: after entering the VD station, the ladle is covered and a hydrogen-inert gas mixture with a hydrogen ratio of 10 to 50 vol% is blown into the ladle through the bottom air-permeable brick, and multiple bottom blowing holes can be selected for bottom blowing, and the total gas supply intensity is 1000 to 6500 NL / t 钢 / min, the blowing time is 10~35min; when the blowing starts, the vacuum pump is turned on to draw the vacuum, and the vacuum degree of the vacuum chamber is below 2kPa; when the blowing ends, the vacuum degree of the vacuum chamber is adjusted to ≤67Pa, and the bottom blowing air brick is used to blow argon into the molten steel to assist in degassing, and the total argon strength is 1000~3000NL / t 钢 / min, argon blowing time 6 to 10min; VD station requires molten steel temperature to be 1600 to 1620℃, molten steel [C] content ≤ 12×10 -6 , [O] content ≤ 10×10 -6 , [P] content ≤ 110×10 -6 , [N] content ≤ 20 × 10 -6 , [H] content ≤ 2.5 × 10 -6 , [S] content ≤ 35 × 10 -6 .

[0018] As a preferred solution of the high-cleanliness IF steel production process described in the present invention, the amount of alloy to be added is calculated according to the VD steel liquid composition; after the alloy is added, soft blowing is performed for 5 to 10 minutes to ensure uniform composition of the steel liquid; after alloying, the temperature of the steel liquid is required to be controlled at 1585 to 1605°C, and the [C] content in the steel liquid is ≤15×10 -6 , [Si] content ≤ 60×10 -6 , [Mn] content is (800~1200)×10 -6, [P] content ≤ 110×10 -6 , [S] content ≤ 40 × 10 -6 , [Ti] content ≤ 120×10 -6 , [Als] content ≤ 10×10 -6 , [O] content ≤ 15×10 -6 , [N] content ≤ 25 × 10 -6 , [H] content ≤ 2.5 × 10 -6 .

[0019] As a preferred solution of the high-cleanliness IF steel production process described in the present invention, wherein: protective casting measures are adopted in continuous casting to strictly prevent secondary oxidation of molten steel and control the temperature of the tundish at 1552-1566°C; ultra-low carbon covering agent is used as the crystallizer covering agent, and protective casting is performed during the entire continuous casting process, and the process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .

[0020] The beneficial effects of the present invention are as follows:

[0021] The present invention proposes a high-cleanliness IF steel production process, which uses RH+VD dual control, uses RH to decarburize molten steel, adds top slag modifier after RH is broken, and sends it into a VD furnace for bottom-blowing hydrogen deoxidation and alloying, and no deoxidized alloy is used in the process. The present invention separates decarburization and deoxidation, thereby avoiding the safety hazard caused by the coexistence of hydrogen and oxygen, and can perform efficient pre-deoxidation of the top slag through a stronger molten pool stirring capacity, and at the same time, deoxidizes by bottom-blowing reducing gas, which not only reduces the oxygen content, but also avoids the risk of secondary oxidation of the molten steel by the slag. At the same time, the residual hydrogen and nitrogen are removed by relying on the degassing capacity of VD. The present invention can reduce safety hazards, improve the cleanliness of the molten steel, and improve the alloy yield, thereby realizing the production of high-cleanliness IF steel. DETAILED DESCRIPTION

[0022] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The invention provides a high-cleanliness IF steel production process, in which only decarburization (oxygen blowing forced deep decarburization and natural decarburization) process is performed in RH; top slag reforming pre-deoxidation is performed after RH leaves the station, and then reducing gas pre-deoxidation is performed in VD, and then H, N and other gas elements are removed under vacuum; the method of the invention avoids the presence of hydrogen and oxygen in the same reactor, and reduces the risk of explosion caused by excessive gas concentration; top slag pre-deoxidation reforming is performed after RH leaves the station, and the secondary oxidation of slag to molten steel is avoided by rapidly and evenly blowing slag components through bottom blowing; the addition of VD can be used to Desulfurizers such as CaO and Mg reduce the desulfurization burden of the KR desulfurization station; H2O bubbles generated by hydrogen injection and argon gas blown at the bottom effectively float inclusions such as slag rolls in the molten steel; all added alloys are used for alloying, reducing the amount of alloy used, saving energy consumption and carbon emissions in the alloy production process; the cleanliness of the molten steel is significantly improved, which is beneficial to the improvement of the mechanical properties of the steel; the reduction of slag basicity increases the life of the furnace lining and refractory materials, reduces problems such as slag rolls, and increases the life of the ladle; the improvement of steel cleanliness helps to make the car lighter.

[0024] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0025] Example 1

[0026] This embodiment is a high-cleanliness IF steel production process, comprising the following steps:

[0027] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 40×10 -6 .

[0028] (2) The scrap steel ratio in the converter was controlled to be 18%; the FeO content in the slag was maintained at 15wt% in the middle of blowing and 18wt% in the slag at the end of blowing; the final converter temperature was controlled at 1699°C, the molten steel volume was 202t, and the final [C] content was controlled at 320×10 -6 The end point [P] content was 93×10 -6 The final [S] content is 40×10 -6 , the end point [O] content is 735×10 -6 ; Steel is tapped using a carbon-free ladle; 505kg of lime is added during steel tapping.

[0029] (3) Drive the ladle car to the RH station, measure the temperature to 1688°C, and set the oxygen to 680×10 -6 , the riser and downcomer of the RH vacuum device are immersed in the molten steel, and the vacuum is started to start the circulation; the five-stage vacuum pump is used to vacuum to 50kPa, and the four-stage pump is started to continue vacuuming to 10kPa to maintain the vacuum degree; the lower oxygen gun starts forced decarburization, and the oxygen supply intensity is 2200NL / t 钢 / min, oxygen blowing time is 11min; start the third-stage pump, second-stage pump, and first-stage pump in sequence, each stage pump is maintained for 1min after being turned on, and the vacuum degree of the vacuum chamber is 67Pa after the last stage pump is turned on, and the vacuum degree is maintained for 7min for natural decarbonization; break the air and leave the station, the exit [C] content is 7×10 -6 , [O] content is 452×10 -6 , the molten steel temperature is 1671℃.

[0030] (4) After RH leaves the station, 96 kg of aluminum-containing top slag modifier is added, the CaO / Al2O3 of the top slag is controlled at 1.5, and the FeO+MnO is controlled at 10 wt%; and it is sent to the VD station.

[0031] (5) After entering the VD station, the ladle is covered and a hydrogen-argon mixed gas with a hydrogen content of 30 vol% is blown in through the three air-permeable bricks at the bottom. The total gas supply intensity is 5400 NL / t 钢 / min, the blowing time is 20min; when blowing starts, the vacuum pump is turned on to draw vacuum, and the vacuum degree of the vacuum chamber is below 2kPa; when blowing ends, the vacuum degree of the vacuum chamber is adjusted to 60Pa, and argon is blown into the molten steel using three bottom-blowing air-permeable bricks to assist in degassing, with a total argon intensity of 2400NL / t 钢 / min, argon blowing time 8min; VD outlet molten steel temperature is 1619℃, molten steel [C] content is 12×10 -6 , [O] content is 9×10 -6 , [P] content 95×10 -6 , [N] content 18×10 -6 , [H] content 2×10 -6 , [S] content 38×10 -6 The amount of alloy to be added is calculated based on the VD steel liquid composition; after the alloy is added, soft blowing is performed for 6 minutes to ensure uniform composition of the steel liquid; after alloying, the temperature of the steel liquid is controlled at 1592°C, and the [C] content in the steel liquid is 13×10 -6 , [Si] content is 52×10 -6 , [Mn] content is 952×10 -6 , [P] content is 85×10 -6 , [S] content is 32×10 -6 , [Ti] content is 110×10 -6 , [Als] content is 9×10 -6 , [O] content is 12×10 -6 , [N] content is 22×10 -6 , [H] content is 2×10 -6 .

[0032] (6) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1558-1566°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .

[0033] The ingot prepared in Example 1 was sampled, and the inclusions in the sample were detected by using the ASPEX inclusion automatic scanning system. The number density of inclusions larger than 1 μm was found to be 5.8 / mm. 2 , the average size of inclusions is 1.6μm.

[0034] Example 2

[0035] This embodiment is a high-cleanliness IF steel production process, comprising the following steps:

[0036] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 36×10 -6 .

[0037] (2) The scrap steel ratio in the converter was controlled to be 20%; the FeO content in the slag was maintained at 14wt% in the middle of blowing and 18wt% in the slag at the end of blowing; the final converter temperature was controlled at 1695℃, the molten steel volume was 152t, and the final [C] content was controlled at 344×10 -6 The end point [P] content is 92×10 -6 , end point [S] content 44×10 -6 The final [O] content is 766×10 -6 ; Steel is tapped using a carbon-free ladle; 380kg of lime is added during steel tapping.

[0038] (3) Drive the ladle car to the RH station, measure the temperature to 1678℃, and set the oxygen to 686×10 -6 , the riser and downcomer of the RH vacuum device are immersed in the molten steel, and the vacuum is started to start the circulation; the five-stage vacuum pump is used to vacuum to 45kPa, and the four-stage pump is started to vacuum to 10kPa to maintain the vacuum degree; the lower oxygen gun starts forced decarburization, and the oxygen supply intensity is 1580NL / t 钢 / min, oxygen blowing time is 14min; start the third-stage pump, second-stage pump, and first-stage pump in sequence, each stage pump is maintained for 1min after being turned on, and the vacuum degree of the vacuum chamber is 67Pa after the last stage pump is turned on, and the vacuum degree is maintained for 8min for natural decarbonization; break the air and exit the station, and the exit requirement [C] content is 12×10 -6 , [O] content is 385×10 -6 , the molten steel temperature is required to be 1667℃.

[0039] (4) After RH leaves the station, 168 kg of aluminum-containing top slag modifier is added, CaO / Al2O3 is controlled at 1.4, and FeO+MnO is controlled at 10 wt%; and it is sent to the VD station.

[0040] (5) After entering the VD station, the ladle is covered and a hydrogen-argon mixed gas with a hydrogen content of 20 vol% is blown in through the two air-permeable bricks at the bottom. The total gas supply intensity is 4400 NL / t 钢 / min, the blowing time is 23min; when blowing starts, the vacuum pump is turned on to draw vacuum, and the vacuum degree of the vacuum chamber is below 2kPa; when blowing ends, the vacuum degree of the vacuum chamber is adjusted to 67Pa, and argon is blown into the molten steel using two bottom-blowing air-permeable bricks to assist in degassing, and the total argon strength is 2200NL / t 钢 / min, argon blowing time 9min; VD outlet molten steel temperature is 1620℃, molten steel [C] content is 12×10 -6 , [O] content is 10×10 -6 , [P] content ≤ 96 × 10 -6 , [N] content 19×10 -6 , [H] content 2.5×10 -6 , [S] content 41×10 -6 The amount of alloy to be added is calculated based on the VD steel liquid composition; after the alloy is added, soft blowing is performed for 6 minutes to ensure uniform composition of the steel liquid; after alloying, the temperature of the steel liquid is controlled at 1597°C, and the [C] content in the steel liquid is 14×10 -6 , [Si] content is 54×10 -6 , [Mn] content is 866×10 -6 , [P] content is 104×10 -6 , [S] content is 34×10 -6 , [Ti] content is 103×10 -6 , [Als] content is 8×10 -6 , [O] content is 14×10 -6 , [N] content is 24×10 -6 , [H] content is 2.5×10 -6 .

[0041] (6) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1555-1564°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .

[0042] The ingot prepared in Example 2 was sampled and the inclusions in the sample were detected by using the ASPEX inclusion automatic scanning system. The number density of inclusions larger than 1 μm was found to be 6.6 / mm. 2 , the average size of inclusions is 2μm.

[0043] Comparative Example 1

[0044] This comparative example is a production process for RH vacuum carburizing and deoxidation of IF steel, comprising the following steps:

[0045] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 42×10 -6 .

[0046] (2) The scrap steel ratio in the converter was controlled to be 19%; the FeO content in the slag was maintained at 17wt% in the middle of blowing and 22wt% in the slag at the end of blowing; the tapping temperature of the converter was 1708℃, the amount of molten steel was 154t, and the final [C] content was controlled at 212×10 -6 The end point [P] content is 91×10 -6 , end point [S] content 44×10 -6 The final [O] content is 920×10 -6 The molten steel is not deoxidized when entering the ladle, and no alloy or carburizer is added. 310 kg of lime is added when the steel is discharged.

[0047] (3) RH arrived at the station, the temperature was 1665℃, and the oxygen content was 894×10 -6 RH vacuuming, open circulation, rising pipe argon blowing intensity at 6500NL / t 钢 / min, a five-stage vacuum pump was used to evacuate to 50 kPa, and a four-stage pump was started to evacuate to 10 kPa to maintain the vacuum degree; 83 kg of a carburizer containing 92% carbon was added to the molten steel; after the carburizer was added to RH, the three-stage pump, the two-stage pump, and the one-stage pump were started in sequence, and each stage of the pump was maintained for 1 minute after being turned on. After the last stage of the pump was turned on, the vacuum degree of the vacuum chamber was 67 Pa, and the molten steel circulated for 10 minutes for deep decarburization; after the decarburization was completed, the oxygen content was determined, and the [O] content was 220×10 -6 , [C] content 29×10 -6 ; 38kg of aluminum particles were added for deoxidation, and alloy was added according to the RH steel alloy content. After the alloy was added, soft blowing was performed for 6 minutes to ensure uniform composition of the molten steel; after alloying, the temperature of the molten steel was controlled at 1586℃, and the [C] content in the molten steel was 30×10 -6 , [Si] content is 52×10 -6 , [Mn] content is 912×10 -6 , [P] content is 93×10 -6 , [S] content is 45×10 -6, [Ti] content is 103×10 -6 , [Als] content is 210×10 -6 , [O] content is 23×10 -6 , [N] content is 27×10 -6 , [H] content is 2×10 -6 .

[0048] (6) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1557-1565°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .

[0049] The ingots prepared in Comparative Example 1 were sampled and the inclusions in the samples were detected by using the ASPEX inclusion automatic scanning system. The statistical result showed that the number density of inclusions larger than 1 μm was 13.4 / mm. 2 , the average size of inclusions is 4.8μm.

[0050] Comparative Example 2

[0051] This comparative example is an IF steel RH+VD production process, comprising the following steps:

[0052] (1) KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be 42×10 -6 .

[0053] (2) The scrap steel ratio in the converter was controlled to be 19%; the FeO content in the slag was maintained at 15wt% in the middle of blowing and 19wt% in the slag at the end of blowing; the final converter temperature was controlled at 1697℃, the molten steel volume was 206t, and the final [C] content was controlled at 314×10 -6 The end point [P] content is 95×10 -6 , end point [S] content 45×10 -6 The final [O] content is 802×10 -6 ; Steel is tapped using a carbon-free ladle; 553kg of lime is added during steel tapping.

[0054] (3) Drive the ladle car to the RH station, measure the temperature to 1683℃, and set the oxygen to 731×10 -6 , the riser and downcomer of the RH vacuum device are immersed in the molten steel, and the vacuum is started to start the circulation; the five-stage vacuum pump is used to vacuum to 50kPa, and the four-stage pump is started to continue vacuuming to 10kPa to maintain the vacuum degree; the lower oxygen gun starts forced decarburization, and the oxygen supply intensity is 1000NL / t 钢 / min, oxygen blowing time is 14min; start the third-stage pump, second-stage pump, and first-stage pump in sequence, each stage pump is maintained for 1min after being turned on, and the vacuum degree of the vacuum chamber is 80Pa after the last stage pump is turned on, and the vacuum degree is maintained for 5min for natural decarbonization; break the air and leave the station, the exit [C] content is 23×10 -6 , [O] content is 472×10 -6 , the molten steel temperature is 1671℃.

[0055] (4) After RH leaves the station, 124 kg of aluminum-containing top slag modifier is added, the CaO / Al2O3 of the top slag is controlled at 1.5, and the FeO+MnO is controlled at 10 wt%; and it is sent to the VD station.

[0056] (5) After entering the VD station, the ladle is covered and a hydrogen-argon mixed gas with a hydrogen content of 30 vol% is blown in through the three air-permeable bricks at the bottom. The total gas supply intensity is 6900 NL / t 钢 / min, the blowing time is 18min; when blowing starts, the vacuum pump is turned on to draw vacuum, and the vacuum degree of the vacuum chamber is below 2kPa; when blowing ends, the vacuum degree of the vacuum chamber is adjusted to 67Pa, and argon is blown into the molten steel using three bottom-blowing air-permeable bricks to assist in degassing, with a total argon intensity of 2700NL / t 钢 / min, argon blowing time 6min; VD outlet molten steel temperature is 1608℃, molten steel [C] content is 23×10 -6 , [O] content is 9×10 -6 , [P] content 98×10 -6 , [N] content 18×10 -6 , [H] content 4.5×10 -6 , [S] content 44×10 -6 The amount of alloy to be added is calculated based on the VD steel liquid composition; after the alloy is added, soft blowing is performed for 7 minutes to ensure uniform steel liquid composition; after alloying, the temperature of the steel liquid is controlled at 1594°C, and the [C] content in the steel liquid is 25×10 -6 , [Si] content is 55×10 -6 , [Mn] content is 954×10 -6 , [P] content is 98×10 -6 , [S] content is 44×10 -6 , [Ti] content is 113×10 -6 , [Als] content is 10×10 -6 , [O] content is 10×10 -6 , [N] content is 23×10 -6 , [H] content is 4×10 -6 .

[0057] (6) Protective casting measures are taken during continuous casting to strictly prevent secondary oxidation of molten steel and control the tundish temperature at 1553-1564°C; ultra-low carbon covering agent is used for the crystallizer covering agent, and protective casting is performed throughout the continuous casting process. The process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .

[0058] The ingots prepared in Comparative Example 1 were sampled and the inclusions in the samples were detected by using the ASPEX inclusion automatic scanning system. The statistical result showed that the number density of inclusions larger than 1 μm was 7.9 / mm. 2 , the average size of inclusions is 2.9μm.

[0059] The present invention uses RH+VD dual control, uses RH to decarburize the molten steel, adds a top slag modifier after RH is broken, and sends it into a VD furnace for bottom-blowing hydrogen deoxidation and alloying, and no deoxidized alloy is used in the process. The present invention separates decarburization and deoxidation to avoid the safety hazards caused by the coexistence of hydrogen and oxygen, and can perform efficient pre-deoxidation of the top slag through a stronger molten pool stirring capacity, and at the same time, bottom-blowing reducing gas for deoxidation, which not only reduces the oxygen content, but also avoids the risk of secondary oxidation of the molten steel by the slag. At the same time, the degassing capacity of VD is relied on to remove residual hydrogen and nitrogen. The present invention can reduce safety hazards, improve the cleanliness of the molten steel, and improve the alloy yield, thereby realizing the production of high-cleanliness IF steel.

[0060] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A high-cleanliness IF steel production process, characterized in that: Through RH+VD dual control, RH is used for decarburization of molten steel. After RH is broken, top slag modifier is added and sent to the VD furnace for bottom blowing hydrogen deoxidation and alloying. No deoxidizing alloy is used in the process.

2. The high-cleanliness IF steel production process according to claim 1, characterized in that: The production process specifically includes: KR pretreatment, converter smelting, RH, VD, and continuous casting.

3. The high-cleanliness IF steel production process according to claim 2, characterized in that: KR pretreatment is used for hot metal desulfurization, and the [S] content in the hot metal after treatment is required to be ≤40×10 -6 .

4. The high-cleanliness IF steel production process according to claim 2, characterized in that: The scrap steel ratio of converter smelting is controlled to be ≤20%; the FeO content in the slag is maintained at ≥15wt% in the middle of blowing, and the FeO content in the slag is ≤20wt% at the end of blowing; the converter terminal temperature is required to be controlled at 1690~1710℃, and the terminal [C] content is controlled at (300~450)×10 -6 , end point [P] content ≤ 100 × 10 -6 , end point [S] content ≤ 50 × 10 -6 , end point [O] content ≥500×10 -6 ; Steel is tapped using a carbon-free ladle; 1-3 kg / t of steel is added 钢 of lime.

5. The high-cleanliness IF steel production process according to claim 2, characterized in that: Drive the ladle car to the RH station, immerse the riser and downcomer of the RH vacuum device in the molten steel, start vacuuming and start circulation; use a five-stage vacuum pump to vacuum to 40-60kPa and maintain for 3-5 minutes, start the four-stage pump to vacuum to 5-15kPa and maintain the vacuum degree; start forced decarburization with the lower oxygen lance, and the oxygen supply intensity is 1200-4500NL / t 钢 / min, oxygen blowing time is 8-15min; start the third-stage pump, second-stage pump, and first-stage pump in sequence, each stage pump is maintained for 1min after being turned on, and after the last stage pump is turned on, the vacuum degree of the vacuum chamber is ≤67Pa, and the vacuum degree is maintained for 6-12min for natural decarbonization; break the air and exit the station, and the exit requirement is [C] content ≤12×10 -6 , the molten steel temperature is required to be 1665~1690℃.

6. The high-cleanliness IF steel production process according to claim 5, characterized in that: Add 0.4~1.5kg / t of RH after leaving the station 钢 The aluminum-containing top slag modifier is used, the top slag basicity is controlled at 1-2, and FeO+MnO is controlled at ≤10wt%; and it is sent to the VD station.

7. The high-cleanliness IF steel production process according to claim 2, characterized in that: After entering the VD station, the ladle is covered and a hydrogen-inert gas mixture with a hydrogen content of 10-50 vol% is blown in through the bottom air bricks. The total gas supply intensity is 1000-6500NL / t 钢 / min, the blowing time is 10~35min; when the blowing starts, the vacuum pump is turned on to draw the vacuum, and the vacuum degree of the vacuum chamber is below 2kPa; when the blowing ends, the vacuum degree of the vacuum chamber is adjusted to ≤67Pa, and the bottom blowing air brick is used to blow argon into the molten steel to assist in degassing, and the total argon strength is 1000~3000NL / t 钢 / min, argon blowing time 6 to 10min; VD station requires molten steel temperature to be 1600 to 1620℃, molten steel [C] content ≤ 12×10 -6 , [O] content ≤ 10×10 -6 , [P] content ≤ 110×10 -6 , [N] content ≤ 20 × 10 -6 , [H] content ≤ 2.5 × 10 -6 , [S] content ≤ 35 × 10 -6 .

8. The high-cleanliness IF steel production process according to claim 7, characterized in that: The amount of additional alloy is calculated based on the VD steel liquid composition; soft blowing for 5 to 10 minutes after the alloy is added to ensure uniform steel liquid composition; after alloying, the steel liquid temperature is required to be controlled at 1585 to 1605°C, and the [C] content in the steel liquid is ≤15×10 -6 , [Si] content ≤ 60×10 -6 , [Mn] content is (800~1200)×10 -6 , [P] content ≤ 110×10 -6 , [S] content ≤ 40 × 10 -6 , [Ti] content ≤ 120×10 -6 , [Als] content ≤ 10×10 -6 , [O] content ≤ 15×10 -6 , [N] content ≤ 25 × 10 -6 , [H] content ≤ 2.5 × 10 -6 .

9. The high-cleanliness IF steel production process according to claim 2, characterized in that: The continuous casting adopts protective casting measures to strictly prevent the secondary oxidation of molten steel and control the temperature of the tundish at 1552-1566℃; the crystallizer covering agent adopts ultra-low carbon covering agent, and the whole continuous casting process is carried out with protective casting, and the process requires oxygen addition of less than 3×10 -6 , nitrogen addition is less than 3×10 -6 .

Citation Information

Patent Citations

  • Process for smelting ultra clean steel by single-nozzle refining furnace

    CN101921895A

  • High-cleanliness pipeline steel smelting process

    CN104630418A

  • Melting method for HIC (Hydrogen Induced Crack)-resistant pipeline steel

    CN109161630A

  • Production method of high-cleanliness bearing steel

    CN113981306A

  • Ultra-low carbon steel smelting continuous casting production process of 100-ton dry VD furnace

    CN115094190A

Cited By

  • High scrap ratio steelmaking nitrogen control integration technology

    CN119685687A

  • High scrap ratio steelmaking nitrogen control integrated technology

    CN119685687B