Cr12MoV steel as well as preparation method and application thereof

Through EBT arc furnace smelting, LF furnace refining and VD furnace refining processes, combined with upsetting forging and gradient heating forging, the problem of poor performance of Cr12 series mold steel is solved, significantly improving the wear resistance and service life of Cr12MoV steel, and meeting the satisfaction of High performance requirements of cold rolls.

CN118910490APending Publication Date: 2024-11-08PANGANG GROUP JIANGYOU CHANGCHENG SPECIAL STEEL COMPANY LIMITED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999940.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing Cr12 series mold steel has poor performance, poor mechanical properties and service performance of cold rolls, making it difficult to meet the requirements of high wear resistance, contact fatigue strength and thermal impact strength.

Method used

EBT arc furnace smelting, LF furnace refining and VD furnace refining technology are adopted, combined with upsetting forging and gradient temperature forging, to control the content of chemical components and non-metallic inclusions, and to reduce eutectic grade and spheroidized tissue segregation through high-temperature homogenization treatment. Improve the uniformity and wear resistance of steel.

Benefits of technology

It significantly improves the wear resistance, contact fatigue strength and thermal impact strength of Cr12MoV steel, extends its service life and meets the demanding working environment requirements of cold rolls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910490A_ABST
    Figure CN118910490A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of Cr12MoV steel, which comprises the following steps: sequentially carrying out EBT electric arc furnace smelting, LF furnace refining and VD furnace refining, pouring to obtain a steel billet, and sequentially carrying out upsetting and drawing forging, annealing, flaw detection, sampling and finishing treatment on the steel billet to obtain the Cr12MoV steel. In the smelting process of the electric arc furnace, the content of C is 1.45%-1.70%, the content of Mo is 0.40%-0.60%, and the content of V is 0.75%-1.00%; the pouring temperature ranges from 1435 DEG C to 1445 DEG C, the ingot body pouring time ranges from 290 s to 370 s, and the riser pouring time ranges from 150 s to 210 s. The invention further discloses the Cr12MoV steel. The invention further discloses the Cr12MoV steel. The invention further discloses an application of the Cr12MoV steel. The high-temperature homogenization treatment is adopted, so that small-particle eutectic carbides in the cast ingot basically disappear, large-particle eutectic carbides are partially dissolved, component segregation is obviously improved, and the carbides in the steel are fine and uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, and in particular to Cr12MoV steel and a preparation method and application thereof. Background Art

[0002] In the past 20 years, my country's mold technology has developed very rapidly, especially in recent years, the demand for molds has been growing rapidly at a rate of 15% per year, and the rapid development of the national economy has put forward higher and higher requirements for mold technology. Cr12 series steel is a high wear-resistant micro-deformation cold working die steel, which is characterized by high wear resistance, hardenability, micro-deformation, high thermal stability, high bending strength, etc. It is an important punching die and cold heading die material, and its consumption ranks first in cold working die steel.

[0003] Die steel is the material used to make dies, and its current status and development reflect a country's industrial level. Cold rolling rolls are subject to great rolling stress during the working process. In addition, problems such as welds, inclusions, and edge cracks in the rolled product can easily lead to instantaneous high temperatures, which can cause strong thermal shocks on the working rolls, resulting in cracks, sticking, peeling, and even scrapping. Therefore, cold rolling rolls must be able to resist cracking and peeling caused by bending stress, torsional stress, and shear stress, and must also have high wear resistance, high contact fatigue strength, high fracture toughness, and thermal shock strength. In order to increase the depth of the hardened layer and the contact fatigue life, reduce the brittleness of the hardened layer and the sensitivity to overheating, and also to meet the further requirements of the rolled product on the mechanical properties and performance of the cold rolling work rolls, the control of trace elements has been increased. Summary of the invention

[0004] The purpose of the present invention is to provide a Cr12MoV steel and a preparation method and application thereof, so as to solve the technical problems in the prior art that the Cr12 series die steel has poor performance and the mechanical properties and use performance of cold rolling rolls are poor.

[0005] To achieve the above object, an embodiment of the present invention provides a method for preparing Cr12MoV steel, comprising sequentially performing EBT arc furnace smelting, LF furnace refining and VD furnace refining, casting to obtain a steel billet, and sequentially performing upsetting forging, annealing, flaw detection, sampling and finishing treatment on the steel billet to obtain Cr12MoV steel;

[0006] During the arc furnace smelting process: the C content is 1.45%-1.70%, the Mo content is 0.40%-0.60%, and the V content is 0.75-1.00%;

[0007] The pouring temperature is 1435℃-1445℃, the ingot pouring time is 290s-370s, and the riser time is 150s-210s.

[0008] One of the preferred solutions of the present invention, EBT electric arc furnace smelting includes:

[0009] The return oxygen blowing method is adopted for smelting. When P in the molten steel after smelting in the EBT electric arc furnace is ≤0.030%, the steel is tapped and the tapping temperature is 1580℃-1630℃.

[0010] One of the preferred solutions of the present invention, LF furnace refining includes the following steps performed in sequence:

[0011] Cooling the molten steel after smelting in the EBT electric arc furnace to a temperature of 1500°C-1530°C;

[0012] After entering the LF furnace for refining, Al wire is fed for deoxidation to make the Al content in the steel 0.05%-0.06%.

[0013] In one of the preferred solutions of the present invention, the charging conditions for LF furnace refining are: C content is 1.1%-1.3%, Cr content is 9.5%-11%, and Si content is 0.2%-0.4%.

[0014] One of the preferred solutions of the present invention, VD furnace refining includes:

[0015] During VD furnace treatment, the vacuum is maintained at an ultimate vacuum of ≤67Pa for 20min-40min.

[0016] In one of the preferred solutions of the present invention, the pouring includes: using argon gas to protect the pouring.

[0017] In one of the preferred solutions of the present invention, the forging adopts a 45MN press for fast forging, and the anvil is preheated before forging, and the total forging ratio of the forging is ≥8.

[0018] In one of the preferred solutions of the present invention, the start forging temperature is ≥1050°C, the final forging temperature is ≥850°C, the forging adopts gradient heating and heat preservation treatment at above 1160°C and repeated upsetting and drawing forging.

[0019] Based on the preparation method of Cr12MoV steel disclosed in the present invention, the present invention also discloses a Cr12MoV steel, which is prepared by the above preparation method. Among the non-metallic inclusions in the Cr12MoV steel, coarse sulfide inclusions are ≤1.5 level, fine sulfide inclusions are ≤1.5 level, coarse oxide inclusions are ≤2.0 level, fine oxide inclusions are ≤2.0 level, coarse silicate inclusions are ≤1.5 level, fine silicate inclusions are ≤1.5 level, coarse spherical oxide inclusions are ≤1.0 level, and fine spherical oxide inclusions are.

[0020] The invention also discloses an application of Cr12MoV steel, which is used as a cold rolling roller.

[0021] In summary, the beneficial effects of the present invention are:

[0022] 1. The Cr12MoV steel of the present invention is produced in accordance with the relevant technical agreement, and the smelting adopts the "electric furnace + AOD + LF++ forging" process technology. Under the premise of ensuring that the chemical composition meets the technical requirements and process internal control requirements, the core technology of 1.9t shaping pouring + forging is adopted. The high-temperature homogenization treatment can basically eliminate the small-grained eutectic carbide in the ingot, partially dissolve the large-grained eutectic carbide, and significantly improve the component segregation, thereby making the carbide in the steel fine and uniform.

[0023] 2. In the preparation method of Cr12MoV steel of the present invention, the eutectic level of the cold rolling roll is reduced, the size of the blocky carbide is reduced, and the flaw detection pass rate is improved by lowering the pouring temperature and extending the pouring time.

[0024] 3. In the preparation method of Cr12MoV steel of the present invention, the forging process adopts gradient heating and heat preservation treatment at above 1160°C and performs repeated upsetting and drawing forging, thereby improving the isotropy of the steel, the uniformity of the composition and spheroidized structure, and refining the grains, which is beneficial to improving the ability to resist crack initiation, thereby significantly improving the service life of the steel.

[0025] 4. The Cr12MoV steel prepared by the present invention is used as a cold rolling roller. The Cr12MoV steel adopts a gradient heating and forging process to reduce the S and P contents, and the high-temperature treatment eliminates the segregation of the spheroidized structure. The performance and wear resistance of the finished product after high-temperature homogenization treatment are significantly better than those of the conventional Cr12MoV cold rolling roller materials used as the basis for research. It has high purity, uniform spheroidized structure, and eutectic carbide unevenness ≤ level 2. It has high toughness and high wear resistance and is suitable for harsh working environments.

[0026] 5. The Cr12MoV steel prepared by the present invention is used as a cold rolling roller, which has high wear resistance, high contact fatigue strength, high fracture toughness and thermal shock strength, and also meets the requirements of the rolled piece on the mechanical properties and performance of the cold rolling working roller. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A forging heating process diagram of an embodiment of the present invention;

[0028] Figure 2 This is a precision forging heating process diagram of an embodiment of the present invention;

[0029] Figure 3 An annealing process diagram of an embodiment of the present invention;

[0030] Figure 4a The electron microscope of the Cr12MoV steel prepared in Example 1 of the present invention is Figure 1 ;

[0031] Figure 4b The electron microscope of the Cr12MoV steel prepared in Example 1 of the present invention is Figure 1 ;

[0032] Figure 5a The electron microscope of the Cr12MoV steel prepared in Example 2 of the present invention is Figure 1 ;

[0033] Figure 5b The electron microscope of the Cr12MoV steel prepared in Example 2 of the present invention is Figure 2 ;

[0034] Figure 6a The electron microscope of the cold-worked steel prepared in the comparative example of the present invention is Figure 1 ;

[0035] Figure 6b The electron microscope of the cold-worked steel prepared in the comparative example of the present invention is Figure 2 . DETAILED DESCRIPTION

[0036] The invention discloses a preparation method of Cr12MoV steel, comprising sequentially performing EBT electric arc furnace smelting, LF furnace refining and VD furnace refining, casting to obtain a steel billet, and sequentially performing upsetting forging, annealing, flaw detection, sampling and finishing treatment on the steel billet to obtain the Cr12MoV steel;

[0037] During the arc furnace smelting process: the C content is 1.45%-1.70%, the Mo content is 0.40%-0.60%, and the V content is 0.75-1.00%;

[0038] The pouring temperature is 1435℃-1445℃, the ingot pouring time is 290s-370s, and the riser time is 150s-210s.

[0039] The Cr12MoV steel of the present invention is produced according to the relevant technical agreement, and the smelting adopts the "electric furnace + AOD + LF++ forging" process technology. Under the premise of ensuring that the chemical composition meets the technical requirements and the process internal control requirements, the core technology of 1.9t shaping pouring + forging is adopted. The high-temperature homogenization treatment can make the small-grained eutectic carbide in the ingot basically disappear, the large-grained eutectic carbide is partially dissolved, and the component segregation is significantly improved, thereby making the carbide in the steel fine and uniform.

[0040] On the basis of ensuring that various components, properties and ultrasonic flaw detection meet the technical requirements, the qualified rate of finished product flaw detection and various properties is guaranteed to be ≥95%.

[0041] Specific, smelting and pouring:

[0042] (1) EBT electric arc furnace smelting includes: adopting return oxygen blowing method to smelt, selecting low P and S cut ends, CrMo return materials and high carbon ferrochrome ingredients, and blowing oxygen temperature to ensure sufficient degassing and removal of inclusions; high temperature steel tapping after satisfying the condition of P≤0.030%, the steel tapping temperature is 1580℃-1630℃; LF furnace conditions: temperature is 1500℃-1530℃, chemical composition C content is 1.1%-1.3%, Cr content is 9.5%-11%, and Si content is 0.2%-0.4%;

[0043] (2) LF furnace refining includes the following steps performed in sequence:

[0044] Cooling the molten steel after smelting in the EBT electric arc furnace to a temperature of 1500°C-1530°C;

[0045] Enter the LF furnace for refining and feed Al wire for deoxidation, so that the Al content in the steel is 0.05%-0.06%;

[0046] Specifically: After the LF furnace enters the tank, 100m of aluminum wire is fed under the thin slag for strong deoxidation. According to the requirements of the refining final slag composition control, refined slag, lime and steel slag are added in batches according to the thickness of the slag entering the tank; after alloying, sampling is fully analyzed, Al is controlled at 0.05%-0.06%, and the chemical composition is adjusted to meet the internal control requirements. After steel is tapped, the slag is removed to a slag thickness of 60mm-100mm. During the slag removal process, pay attention to the argon flow rate to prevent the molten steel from being exposed and inhaled;

[0047] (3) VD furnace refining includes: during VD furnace treatment, the vacuum is maintained at a limit of ≤67Pa for 20min-40min;

[0048] (4) Ladle pouring temperature T = 1435-1445 ° C, pouring time: ingot body time 290s-370s, riser time 150s-210s;

[0049] Ensure the vacuum degree and the ultimate vacuum holding time, blow argon with a large flow rate and strong stirring under the ultimate vacuum degree, fully contact the steel and slag, improve the mass transfer kinetics of Al2O3 inclusions in the steel, reduce the level of B and D type oxide inclusions, and improve the cleanliness of the steel. Among them, B type oxides include chain oxide inclusions, and D type oxides include point-like non-deformed oxide inclusions;

[0050] Pouring: argon protection is used during pouring, the soft argon blowing time is 32 minutes, and pouring is performed when the temperature reaches the hanging bag temperature; argon protection is used during pouring to control the gas content in the steel. The steel billet is sequentially subjected to upsetting, forging, annealing, flaw detection, sampling and finishing treatment to obtain cold working die steel;

[0051] The current ladle pouring temperature is T = 1435℃1445℃, pouring time: ingot body time 290 S-370 S , riser time 150 S -210 S ; The previous hanging ladle pouring temperature: 1445℃-1455℃, pouring time control: ingot body time 260s-380s, riser time 130-220s). The present invention reduces the eutectic level, reduces the size of blocky carbides, and improves the flaw detection pass rate by lowering the pouring temperature and extending the pouring time;

[0052] ① Alloy element control: C content is controlled at 1.45%-1.70% to reduce the aggregation of C content; Mo content is controlled at 0.40%-0.60% to improve the hardenability of this steel; V content is controlled at 0.75-1.00% to refine the structure and grain;

[0053] ② Reduce the pouring temperature of the steel to reduce segregation;

[0054] ③ Improve purity and reduce gas content in steel ingots, O content ≤15ppm, N content ≤150ppm;

[0055] (5) Forging includes: the anvil must be preheated to 200℃-250℃ before forging (or use a hot anvil after forging), and it is strictly forbidden to use a cold anvil; forging process such as Figure 1 As shown, the starting forging temperature is ≥1050℃, the final forging temperature is ≥850℃, the edges are squared and chamfered, and cracks are removed as soon as possible; the forging method of "two light and one heavy" should be strictly followed during the operation, with light pressure at the beginning and end of forging and heavy pressure in the middle. During the forging process, attention should be paid to uniform deformation of each part and uniform temperature of each part; when the edges and corners become dark, the forging should be stopped and the furnace should be returned in time, and the re-firing time should be ≥2h; the electric hydraulic hammer should be used to cut the cap of the octagonal billet and turn to fine forging when it is completely red, and the size of the fine forging billet should be considered according to the reserved deformation of ≥40% of the finished material;

[0056] Precision forging heating process:

[0057] 1) The hot-rolled blank of the press is put into the furnace and kept at 1140±20℃ for ≥2h before forging;

[0058] 2) Cold billet heating process of precision forging machine Figure 2 As shown;

[0059] (6) Finished product annealing process: Finished product annealing process such as Figure 3 shown.

[0060] The present invention adopts gradient heating and heat preservation treatment at above 1160°C and performs repeated upsetting and drawing forging, thereby improving the isotropy of steel, the uniformity of composition and spheroidized structure, refining grains, and being beneficial to improving the ability to resist crack initiation, thereby significantly improving the service life of the steel. The gradient heating and forging process (the above process) is adopted to reduce the S and P contents, and the high temperature treatment eliminates the segregation of spheroidized structure. The performance and wear resistance of the finished product after high temperature homogenization treatment are significantly better than the conventional Cr12MoV cold rolling roller material as the research basis, with high purity, uniform spheroidized structure, eutectic carbide unevenness ≤ 2 levels, high toughness and high wear resistance, and suitable for harsh working environments.

[0061] The present invention also discloses a Cr12MoV steel, which is prepared by the above-mentioned preparation method. Among the non-metallic inclusions in the Cr12MoV steel, coarse sulfide inclusions are ≤1.5 level, fine sulfide inclusions are ≤1.5 level, coarse oxide inclusions are ≤2.0 level, fine oxide inclusions are ≤2.0 level, coarse silicate inclusions are ≤1.5 level, fine silicate inclusions are ≤1.5 level, coarse spherical oxide inclusions are ≤1.0 level, and fine spherical oxide inclusions are ≤1.0 level.

[0062] The invention also discloses an application of Cr12MoV steel, which is used as a cold rolling roll. The Cr12MoV steel prepared by the invention is used as a cold rolling roll, and the cold rolling roll has high wear resistance, high contact fatigue strength, high fracture toughness and thermal shock strength, and also meets the requirements of the rolled piece on the mechanical properties and use performance of the cold rolling work roll.

[0063] Example 1

[0064] Composition control: The raw material components of the ledeburite cold working die steel are, by mass percentage, C 1.52%, Si 0.23%, Mn 0.40%, S 0.001%, P 0.030%, Cr 11.8%, Mo 0.48% and V 0.25%;

[0065] EBT: adopts return oxygen blowing method for smelting, selects low P, S cut ends, CrMo return materials and high carbon ferrochrome ingredients, and the oxygen blowing temperature is to ensure sufficient degassing and removal of inclusions. After the condition of P≤0.030% is met, the steel is tapped at high temperature, and the tapping temperature is 1590℃-1620℃; the conditions for entering the LF furnace: temperature 1515℃, chemical composition C1.6%, Cr 12%, Si 0.25%;

[0066] LF furnace: After the LF furnace enters the tank, 100m of aluminum wire is fed under the thin slag for strong deoxidation. According to the requirements of the refined final slag composition control, refined slag, lime and steel slag are added in batches according to the thickness of the slag entering the tank. After alloying, samples are taken for full analysis, and Al is controlled at 0.05%-0.06%. The chemical composition is adjusted to meet the internal control requirements. After steel is tapped, the slag is removed to a slag thickness of 65-100mm. During the slag removal process, pay attention to the argon flow rate to prevent the molten steel from being exposed and inhaled;

[0067] VD furnace: During VD treatment, the ultimate vacuum is ≤67Pa and the holding time is 30min;

[0068] Ladle pouring temperature T = 1435℃;

[0069] Ensure the vacuum degree and ultimate vacuum holding time, blow argon with large flow rate and strong stirring under ultimate vacuum degree, fully contact the steel and slag, improve the mass transfer kinetics of Al2O3 inclusions in steel, reduce the level of B and D oxide inclusions, and improve the cleanliness of steel;

[0070] Pouring: argon blowing time is 35min, and pouring is performed when the temperature reaches the ladle temperature; argon protection is used during pouring to control the gas content in the steel. The steel billet is sequentially subjected to upsetting, forging, annealing, flaw detection, sampling and finishing treatment to obtain ledeburite cold working die steel, 150 round, crystal carbide unevenness is 2, such as Figure 4a-4b As shown, according to the SEM electron microscope image, it can be seen that by adopting the process of the present application, the internal structure of the steel is uniform and refined, the small-grained eutectic carbide inside the steel basically disappears, the large-grained eutectic carbide is partially dissolved, and the component segregation is significantly improved, thereby making the carbides in the steel small and uniform.

[0071] Example 2

[0072] Composition control: The raw material components of the ledeburite cold working die steel are, by mass percentage, C 1.55%, Si 0.25%, Mn 0.38%, S 0.001%, P 0.030%, Cr 11.6%, Mo 0.48% and V 0.23%;

[0073] EBT: adopts return oxygen blowing method for smelting, selects low P, S cut ends, CrMo return materials and high carbon ferrochrome ingredients, and the oxygen blowing temperature is to ensure sufficient degassing and removal of inclusions. After the condition of P≤0.030% is met, the steel is tapped at high temperature, and the tapping temperature is 1590℃-1620℃; the conditions for entering the LF furnace: temperature 1518℃, chemical composition C1.58%, Cr 11.9%, Si 0.28%;

[0074] LF furnace: After the LF furnace enters the tank, aluminum wire 100m / furnace is fed under the thin slag for strong deoxidation, and refined slag, lime and steel slag are added in batches according to the slag thickness in the tank according to the requirements of the final slag composition control. After alloying, sampling is fully analyzed, Al is controlled at 0.05%-0.06%, and the chemical composition is adjusted to meet the internal control requirements. After steel is tapped, the slag is removed to a slag thickness of 65mm-100mm. During the slag removal process, pay attention to the argon flow rate to prevent the steel liquid from being exposed and inhaled.

[0075] VD furnace: During VD treatment, the ultimate vacuum is ≤68Pa and the holding time is 32min;

[0076] Ladle pouring temperature T = 1437℃;

[0077] Ensure the vacuum degree and ultimate vacuum holding time, blow argon with large flow rate and strong stirring under ultimate vacuum degree, fully contact the steel and slag, improve the mass transfer kinetics of Al2O3 inclusions in steel, reduce the level of B and D oxide inclusions, and improve the cleanliness of steel;

[0078] Pouring: Soft argon blowing time is 35 minutes, and pouring is performed when the temperature reaches the ladle temperature. During pouring, argon protection is used to control the gas content in the steel. The steel billet is sequentially subjected to upsetting, forging, annealing, flaw detection, sampling and finishing treatment to obtain ledeburite cold working die steel, 180 round, carbide unevenness is 2, such as Figure 5a-5b As shown, according to the SEM electron microscope image, it can be seen that by adopting the process of the present application, the internal structure of the steel is uniform and refined, the small-grained eutectic carbide inside the steel basically disappears, the large-grained eutectic carbide is partially dissolved, and the component segregation is significantly improved, thereby making the carbides in the steel small and uniform.

[0079] Comparative Example

[0080] Composition control: The raw material components of the ledeburite cold working die steel are, by mass percentage, C 1.52%, Si 0.23%, Mn 0.40%, S 0.001%, P 0.030%, Cr 11.8%, Mo 0.48% and V 0.25%;

[0081] EBT: adopts return oxygen blowing method for smelting, selects low P, S cut head, CrMo return material and high carbon ferrochrome ingredients, and the oxygen blowing temperature is to ensure sufficient degassing and removal of inclusions. After meeting the condition of P≤0.030%, high temperature steel is tapped, and the tapping temperature is 1590-℃1620℃; LF furnace conditions: temperature 1525℃, chemical composition C1.57%, Cr 11.8%, Si 0.36%;

[0082] LF furnace: After the LF furnace enters the tank, 100m of aluminum wire is fed under the thin slag for strong deoxidation. According to the requirements of the final slag composition control, refined slag, lime and steel slag are added in batches according to the thickness of the slag entering the tank. After alloying, samples are taken for full analysis, and Al is controlled at 0.05%-0.06%. The chemical composition is adjusted to meet the internal control requirements. After steel is tapped, the slag is removed to a slag thickness of 65mm-100mm. During the slag removal process, pay attention to the argon flow rate to prevent the molten steel from being exposed and inhaled;

[0083] VD furnace: During VD treatment, the ultimate vacuum is ≤70Pa and the holding time is 34min;

[0084] Ladle pouring temperature T = 1453℃;

[0085] Ensure the vacuum degree and ultimate vacuum holding time, blow argon with large flow rate and strong stirring under ultimate vacuum degree, fully contact the steel and slag, improve the mass transfer kinetics of Al2O3 inclusions in steel, reduce the level of B and D oxide inclusions, and improve the cleanliness of steel;

[0086] Pouring: 40 minutes of soft argon blowing time, pouring when the temperature reaches the ladle temperature. During pouring, argon protection is used to control the gas content in the steel. The steel billet is sequentially subjected to upsetting, forging, annealing, flaw detection, sampling and finishing treatment to obtain ledeburite cold working die steel, 180 round, eutectic carbide unevenness is 4, 3.5, such as Figure 6a-6b As shown, according to the SEM electron microscope image, it can be seen that when the original process is used, the internal structure uniformity of the steel is poor, the small particles of eutectic carbides inside the steel are aggregated, the large particles of eutectic carbides are partially not dissolved, and the composition segregation is serious.

[0087] Data processing

[0088] Table 1: Non-metallic inclusion content of Cr12MoV steel obtained in Examples 1-2 and Comparative Examples

[0089]

[0090] Combined with Figure 4a-6b The process of the present application can make the small-grain eutectic carbide in the ingot basically disappear, the large-grain eutectic carbide partially dissolve, and the component segregation significantly improve, thereby making the carbides in the steel small and uniform.

[0091] At the same time, according to the data in Table 1, it can be seen that through process improvement, the eutectic level is reduced, the size of blocky carbides is reduced, and the flaw detection pass rate is improved.

[0092] The embodiments described above are merely descriptions of preferred implementations of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary engineering and technical personnel in the field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing Cr12MoV steel, characterized in that: The method comprises the following steps: performing EBT electric arc furnace smelting, LF furnace refining and VD furnace refining in sequence, casting to obtain a steel billet, and performing upsetting and forging, annealing, flaw detection, sampling and finishing treatment in sequence to obtain Cr12MoV steel; During the arc furnace smelting process: the C content is 1.45%-1.70%, the Mo content is 0.40%-0.60%, and the V content is 0.75-1.00%; The pouring temperature is 1435° C.-1445° C., the ingot pouring time is 290s-370s, and the riser time is 150s-210s.

2. The method for preparing Cr12MoV steel according to claim 1, characterized in that: The EBT electric arc furnace smelting includes: The return oxygen blowing method is adopted for smelting. When P in the molten steel after smelting in the EBT electric arc furnace is ≤0.030%, the steel is tapped and the tapping temperature is 1580℃-1630℃.

3. The method for preparing Cr12MoV steel according to claim 1, characterized in that: The LF furnace refining comprises the following steps which are performed in sequence: Cooling the molten steel after smelting in the EBT electric arc furnace to a temperature of 1500°C-1530°C; After entering the LF furnace for refining, Al wire is fed for deoxidation to make the Al content in the steel 0.05%-0.06%.

4. A method for preparing Cr12MoV steel as claimed in claim 3, characterized in that: The feeding conditions of the LF furnace refining are: the C content is 1.1%-1.3%, the Cr content is 9.5%-11%, and the Si content is 0.2%-0.4%.

5. The method for preparing Cr12MoV steel according to claim 1, characterized in that: The VD furnace refining includes: During VD furnace treatment, the vacuum is maintained at an ultimate vacuum of ≤67Pa for 20min-40min.

6. The method for preparing Cr12MoV steel according to claim 1, characterized in that: The pouring comprises: using argon gas to protect the pouring.

7. The method for preparing Cr12MoV steel according to claim 1, characterized in that: The forging adopts 45MN press fast forging, and the anvil is preheated before forging, and the total forging ratio of the forging is ≥8.

8. A method for preparing Cr12MoV steel as claimed in claim 1 or 7, characterized in that: The forging start temperature is ≥1050°C, the final forging temperature is ≥850°C, the forging adopts gradient heating and heat preservation treatment at above 1160°C and repeated upsetting and drawing forging.

9. A Cr12MoV steel, characterized in that: The Cr12MoV steel is prepared by the preparation method described in any one of claims 1 to 8, wherein among the non-metallic inclusions in the steel, coarse sulfide inclusions are ≤1.5 level, fine sulfide inclusions are ≤1.5 level, coarse oxide inclusions are ≤2.0 level, fine oxide inclusions are ≤2.0 level, coarse silicate inclusions are ≤1.5 level, fine silicate inclusions are ≤1.5 level, coarse spherical oxide inclusions are ≤1.0 level, and fine spherical oxide inclusions are.

10. An application of the Cr12MoV steel according to claim 9, characterized in that: Used as cold rolling roller.