Production and preparation method of rare-earth high-strength corrosion-resistant 500MPa Z-shaped steel

Through the chemical composition design of rare earth element microalloyation and VN microalloyation, combined with optimized steelmaking and steel rolling processes, the comprehensive performance problems of high strength, corrosion resistance and low temperature toughness of railway steel are solved, and high strength and corrosion resistance are achieved. and low-weight steel production meets the performance requirements of high-speed heavy-load transportation.

CN118910495APending Publication Date: 2024-11-08BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411185570.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to achieve comprehensive performance of high strength, corrosion resistance and low weight in railway steel at the same time, especially under low temperature conditions, and the corrosion resistance and toughness of the steel are not sufficient to meet the needs of high-speed heavy-load transportation.

Method used

The chemical composition design of rare earth elements is adopted, combined with VN microalloyation, and optimizes the chemical composition and physical properties of steel materials by controlling steelmaking and rolling process parameters such as molten pretreatment, superheat control, rolling temperature and time. Ensure that the yield strength, tensile strength, elongation and corrosion resistance of the steel meet the index of 500MPa, 610MPa, 20% and 46J.

Benefits of technology

The high strength, corrosion resistance and low temperature toughness of steel are achieved, and the performance indicators of 500MPa yield strength, 610MPa tensile strength and 20% elongation are met. At the same time, the low temperature impact performance at -40℃ reaches 100J, which significantly improves the overall performance of steel. and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013391000000051
    Figure BDA0005013391000000051
  • Figure BDA0005013391000000061
    Figure BDA0005013391000000061
  • Figure BDA0005013391000000062
    Figure BDA0005013391000000062
Patent Text Reader

Abstract

The invention discloses a production and preparation method of rare-earth high-strength corrosion-resistant 500MPa Z-shaped steel. The production and preparation method comprises a steelmaking process flow and a steel rolling process flow, the chemical components are as follows: 0.10%-0.12% of C; 0.40% to 0.50% of Si; mn: 1.30% to 1.40%; p: less than or equal to 0.010%; s: less than or equal to 0.008%; 0.30% to 0.35% of Cu; 0.35% to 0.45% of Ni; 0.40% to 0.50% of Cr; 0.10% to 0.12% of V; rE: 0.0030% to 0.0060%, and N: 0.012% to 0.015%; and 0.020 to 0.040 percent of Al. The performance indexes of the steel plate meet the requirements that the yield strength Rel is larger than or equal to 500 MPa, the tensile strength Rm is larger than or equal to 610 MPa, the ductility A is larger than or equal to 20%, and the-40 DEG C low-temperature impact is larger than or equal to 46 J.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material metallurgy, and in particular relates to a production method for a rare earth high-strength and corrosion-resistant 500MPa B-shaped steel. Background Art

[0002] High-strength steel can effectively reduce the cross-sectional area and mass of consumables in buildings. For the same building, the resources and funds spent on using high-strength steel and ordinary-strength steel are quite different. The use of high-strength steel can give full play to the characteristics of components, reduce steel waste, and increase energy utilization. It is the construction foundation and fundamental guarantee for building a resource-saving and environmentally friendly society.

[0003] With the driving force of my country's economic development on railway transportation, railway steel has been continuously developed. As an important type of railway steel, YQ450NQR1 high-strength and high-weathering steel has the characteristics of high strength, corrosion resistance, and low temperature resistance. It is a special steel for making the middle beam of train carriages and an important guarantee for heavy-load trains. Railway transportation is developing in the direction of high speed and heavy load. Heavy-load railway transportation has been paid attention to by railway development in various countries due to its large transportation capacity, high transportation capacity and low transportation cost, especially in some countries with vast territory, rich resources, and a large proportion of coal and ore. At present, in my country's railway freight car transportation, 310 steel is used as the beam of railway freight cars. It is the main load-bearing component of railway freight cars, and the material is mainly YQ450NQR1.

[0004] Rare earth elements in steel can improve the toughness, ductility and corrosion resistance of steel. With the implementation of the country's green, low-carbon and environmental protection policies, improving the strength and corrosion resistance of steel can effectively reduce the weight of the vehicle body, save energy, and have the characteristics of green, low-carbon and environmental protection. Summary of the invention

[0005] The purpose of the present invention is to provide a method for producing rare earth high-strength corrosion-resistant 500MPa B-shaped steel, the performance indicators of which meet the following requirements: yield strength Rel≥500MPa, tensile strength Rm≥610MPa, elongation A≥20%, -40℃ low-temperature impact≥46J, corrosion resistance rate≤1.50g / m 2 .h.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] The invention discloses a method for producing and preparing a rare earth high-strength and corrosion-resistant 500MPa B-shaped steel, comprising: a steelmaking process flow: molten iron - molten iron pretreatment - converter - refining outside the furnace - continuous casting, and a steel rolling process flow: a walking beam heating furnace - high-pressure water dephosphorization - BD primary rolling - CCS finishing rolling - cooling - straightening - sawing - inspection - bundling - storage, and is characterized in that: the technical parameters controlled in the steelmaking process are:

[0008] Use VN alloy with V, N element percentage ≥ 0.01%;

[0009] Continuous casting superheat ≤30℃;

[0010] Casting machine pulling speed 0.60m / min~0.65m / min;

[0011] Crystallizer cooling water temperature ≥26℃;

[0012] The technical parameters controlled in the rolling process are:

[0013] 1) Heating temperature 1200-1250℃, insulation time ≥4 hours;

[0014] 2) Rolling temperature ≤ 1100℃;

[0015] 3) Final rolling temperature ≤ 830℃;

[0016] The chemical composition of the B-shaped steel includes, by weight percentage, the following: C: 0.10%-0.12%; Si: 0.40%-0.50%; Mn: 1.30%-1.40%; P: ≤0.010%; S: ≤0.008%; Cu: 0.30%-0.35%; Ni: 0.35%-0.45%; Cr: 0.40%-0.50%; V: 0.10%-0.12%; RE: 0.0030%-0.0060%, N: 0.012%-0.015%; Al: 0.020%-0.040%, and the rest is Fe and inevitable trace impurities.

[0017] Furthermore, the chemical composition of the B-shaped steel includes, by weight percentage: C: 0.11%; Si: 0.42%; Mn: 1.38%; P: 0.009%; S: 0.005%; Cu: 0.35%; Ni: 0.39%; Cr: 0.44%; V: 0.11%; RE: 0.0045%, N: 0.012%; Al: 0.025%, and the rest is Fe and inevitable trace impurities.

[0018] Furthermore, the chemical composition of the B-shaped steel includes, by weight percentage: C: 0.10%; Si: 0.44%; Mn: 1.35%; P: 0.008%; S: 0.003%; Cu: 0.33%; Ni: 0.42%; Cr: 0.43%; V: 0.11%; RE: 0.0054%, N: 0.013%; Al: 0.030%, and the rest is Fe and inevitable trace impurities.

[0019] Furthermore, the mechanical properties meet the following requirements: yield strength ≥ 550 MPa, tensile strength ≥ 650 MPa, and elongation ≥ 22%.

[0020] Furthermore, the -40°C impact value satisfies: ≥100J.

[0021] The design principle is as follows:

[0022] C: C is the most effective element for improving the strength of steel. As the C content increases, the tensile strength and yield strength of steel increase, but the elongation and impact toughness decrease, the corrosion resistance also decreases, and the heat affected zone of the steel will also be hardened, resulting in the generation of welding cold cracks. In order to ensure that the material has good comprehensive properties, the C content of the steel of the present invention is designed to be 0.10% to 0.12%.

[0023] Mn: Mn is an important toughening element with low composition. With the increase of manganese content, the strength of steel is significantly improved, the processing performance of steel is improved, and the tough-brittle transition temperature hardly changes. However, if the manganese content is too high, it will inhibit the transformation of ferrite, affect the yield strength of steel, and be unfavorable for the control of yield strength ratio. The Mn element content of the material of the present invention is designed to be Mn: 1.30% to 1.40%.

[0024] Si: Si can improve the corrosion resistance of steel and is often added to stainless steel, low alloy steel, and corrosion-resistant alloys to improve the corrosion resistance of these alloys, so that they have the properties of resistance to chloride stress corrosion cracking, pitting corrosion, hot concentrated nitric acid corrosion, oxidation resistance, and seawater corrosion resistance. Studies have shown that in a hot and humid atmospheric environment, Si can significantly improve the atmospheric corrosion resistance of carbon steel and low alloy steel. In addition, Si can also improve the corrosion resistance of low alloy steel in the splash zone of seawater. The Si element content of the material of the present invention is designed to be 0.40% to 0.50%.

[0025] P, S: P and S are impurity elements in steel. P has a certain effect on improving corrosion resistance, but P is an element that is easy to segregate. It will cause serious segregation in some parts of the steel, reduce plasticity and toughness, and is extremely harmful to low-temperature toughness. The S element is easy to segregate and enrich in steel, and is an element that is harmful to corrosion resistance. The steel of the present invention strictly controls the sulfur and phosphorus content levels in terms of metallurgical quality, that is, P: ≤0.010%; S: ≤0.008%.

[0026] V: V has a strong ability to combine with C, O, and N, and forms extremely stable compounds with them, thereby refining the grains, reducing the thermal sensitivity and temper brittleness of steel. It can significantly improve the welding performance of ordinary low-alloy steel. The V content of the steel of the present invention is designed to be 0.10% to 0.12%.

[0027] Cu: Cu has substantially the same function as Ni, and the precipitate of Cu can also improve the high temperature strength and atmospheric corrosion resistance of steel. The Cu content of the steel of the present invention is designed to be 0.30% to 0.35%.

[0028] Ni: Ni is a relatively stable element. Adding Ni can change the self-corrosion potential of steel in a positive direction, thus increasing the stability of steel. In addition, Ni is added mainly to form a Cu-Ni alloy with Cu to prevent the occurrence of "copper embrittlement". Taking all factors into consideration, the control range of Ni content is 0.35% to 0.45%.

[0029] Cr: Cr can improve the strength, hardness and atmospheric corrosion resistance of steel. When added with other alloying elements, the effect is more significant. Chromium can slow down the decomposition rate of austenite, significantly improve the hardenability of steel, and have a secondary hardening effect, but it also increases the temper brittleness tendency of steel. However, when the chromium content is too high, the toughness of the base material and the heat-affected zone will be reduced. The Cr element content of the steel of the present invention is designed to be 0.40% to 0.50%.

[0030] RE:RE has a significant role in purification and modification in steel. The cleanliness of steel is constantly improving, and the microalloying effect of rare earth elements is becoming increasingly prominent. Rare earth microalloying includes solid solution strengthening of trace rare earth elements, the interaction between rare earth elements and other solute elements and compounds, the existence state (atoms, inclusions or compounds), size, morphology and distribution of rare earth elements, especially the segregation at grain boundaries and the influence of rare earth on the surface and matrix structure of steel. Therefore, the RE element content of the steel of the present invention is designed to be 0.0030% to 0.0060%.

[0031] Al: Al has a strong affinity with O and N, and is a deoxidizing and nitrogen fixing agent during steelmaking. Aluminum can strongly reduce the austenite phase region in steel, refine the intrinsic grain size of steel, reduce the notch sensitivity of steel, reduce and eliminate the aging phenomenon of steel, especially reduce the toughness-brittleness transition temperature of steel, and improve the low-temperature toughness of steel. However, when the solid-solution Al content in steel exceeds a certain value, the austenite grains tend to grow and coarsen. The Al element content of the steel of the present invention is designed to be 0.020-0.040%.

[0032] N: Nitrogen can dissolve in steel to form a solid solution. In addition, nitrogen can also form nitrides in steel, which preferentially nucleate in steel and increase the dislocation of ferrite, which can effectively increase the strength and toughness of steel. The N content of the steel of the present invention is designed to be 0.012-0.015%.

[0033] Compared with the prior art, the beneficial technical effects of the present invention are:

[0034] The chemical composition design of low-carbon micro-alloying and adding rare earth elements and the synergistically optimized process give the material good strength, toughness and corrosion resistance.

[0035] VN microalloying is used to utilize the strong bonding ability of V with C, O, and N, forming extremely stable compounds with them to refine the grains of the material. DETAILED DESCRIPTION

[0036] The present invention is further described below by means of specific examples. The examples are only for the purpose of explanation, and the protection scope of the present invention is not limited to these examples.

[0037] The present invention is further described below:

[0038] Tables 1 and 2 show the weight percentage contents of chemical components and carbon equivalents and steelmaking process parameters of various embodiments of the present invention, Table 3 shows the steel rolling process values, and Table 4 shows the test results of the performance of various embodiments.

[0039] Table 1 Chemical composition and weight percentage of each example

[0040]

[0041]

[0042] Table 2 Steelmaking production process parameters of each embodiment

[0043]

[0044] Table 3 Steel rolling process values ​​of various embodiments of the present invention

[0045] Example Heating time Heating temperature ℃ Rolling temperature ℃ Finishing rolling temperature℃ 1 4.5 1210 1030 821 2 4.5 1190 1035 820

[0046] Table 4 shows the test results of the performance of each embodiment.

[0047]

[0048] It can be seen from Table 1 that the chemical composition level steelmaking processes of Examples 1 and 2 are within the scope required by the present invention, and the smelting composition is well controlled.

[0049] Through the test data analysis of Table 3 and Table 4 and the rolling process, all performance indicators of the embodiment meet the technical requirements.

[0050] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for producing rare earth high-strength corrosion-resistant 500MPa B-shaped steel, comprising: Steelmaking process: molten iron - molten iron pretreatment - converter - refining outside the furnace - continuous casting, steel rolling process: walking beam heating furnace - high pressure water dephosphorization - BD primary rolling - CCS finishing rolling - cooling - straightening - sawing - inspection - bundling - storage, characterized in that: the technical parameters controlled in the steelmaking process are: Use VN alloy with V, N element percentage ≥ 0.01%; Continuous casting superheat ≤30℃; Casting machine pulling speed 0.60m / min~0.65m / min; Crystallizer cooling water temperature ≥26℃; The technical parameters controlled in the rolling process are: 1) Heating temperature 1200-1250℃, insulation time ≥4 hours; 2) Rolling temperature ≤ 1100℃; 3) Final rolling temperature ≤ 830℃; The chemical composition of the B-shaped steel includes, by weight percentage, the following: C: 0.10%-0.12%; Si: 0.40%-0.50%; Mn: 1.30%-1.40%; P: ≤0.010%; S: ≤0.008%; Cu: 0.30%-0.35%; Ni: 0.35%-0.45%; Cr: 0.40%-0.50%; V: 0.10%-0.12%; RE: 0.0030%-0.0060%, N: 0.012%-0.015%; Al: 0.020%-0.040%, and the rest is Fe and inevitable trace impurities.

2. The method for producing rare earth high-strength and corrosion-resistant 500MPa B-shaped steel according to claim 1, characterized in that: The chemical composition of the B-shaped steel includes, by weight percentage, C: 0.11%; Si: 0.42%; Mn: 1.38%; P: 0.009%; S: 0.005%; Cu: 0.35%; Ni: 0.39%; Cr: 0.44%; V: 0.11%; RE: 0.0045%, N: 0.012%; Al: 0.025%, and the rest is Fe and inevitable trace impurities.

3. The method for producing rare earth high-strength and corrosion-resistant 500MPa B-shaped steel according to claim 1, characterized in that: The chemical composition of the B-shaped steel includes, by weight percentage, C: 0.10%; Si: 0.44%; Mn: 1.35%; P: 0.008%; S: 0.003%; Cu: 0.33%; Ni: 0.42%; Cr: 0.43%; V: 0.11%; RE: 0.0054%, N: 0.013%; Al: 0.030%, and the rest is Fe and inevitable trace impurities.

4. The method for producing rare earth high-strength and corrosion-resistant 500MPa B-shaped steel according to claim 1, characterized in that: Mechanical properties meet the following requirements: yield strength ≥550MPa, tensile strength ≥650MPa, elongation ≥22%.

5. The method for producing rare earth high-strength and corrosion-resistant 500MPa B-shaped steel according to claim 1, characterized in that: -40℃ impact value meets: ≥100J.

Citation Information

Patent Citations

  • Preparation method of Q460 hot rolled round steel for rare earth low-temperature-resistant automobile part

    CN111500931A

  • Production and preparation method of high-performance Q390GJC hot-rolled H-shaped steel for building

    CN116200652A

  • Preparation method of high-strength, low-temperature-resistant and sulfuric-acid-corrosion-resistant S450AW steel for rail wagons

    CN116377350A

  • Production and preparation method of high-strength and low-temperature-resistant YQ500NQR1 steel for rail wagons