Preparation process of ultraviolet antireflection film and ultraviolet antireflection film
By adopting multi-layer structural technology and fine preparation technology in UV urgency membranes, the problems of vulnerability and low transmittance of traditional membrane layers are solved, and high-performance and long-life UV urgency membranes are achieved, suitable for high temperature and high temperatures Energy UV light applications.
Patent Information
- Application Number
- CN202411107346.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional UV amplitting membranes are prone to damage, have low transmittance and poor thermal stability, and cannot withstand the application of UV continuous pulses and pulsed lasers during long-term use, resulting in limited service life and performance.
Using a top-down multi-layer structure process, including evaporation preparation of alumina layer and silicon oxide layer, combined with ion source cleaning and phased annealing treatment, ensure the cleanliness, density and thermal stability of the film layer, and enhance the film. Durability and optical properties of the layer.
It significantly improves the durability, transmittance and thermal stability of the film layer, extends service life, and adapts to efficient UV light applications in complex environments, providing more reliable and efficient optical components.
Smart Images

Figure CN118910555A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of optical thin films, and in particular to a preparation process of an ultraviolet anti-reflection film and the ultraviolet anti-reflection film. Background Art
[0002] Traditional UV anti-reflection films are mainly made of single-layer magnesium fluoride plating. However, this film has many problems, such as the film is easy to damage and fall off, and the transmittance is relatively low. Especially in the application of UV continuous pulse and pulse laser, the traditional substrate film often cannot withstand long-term use, and cracks or film shedding may occur in a short time. These problems seriously affect the service life and performance of the UV anti-reflection film. Therefore, a new UV anti-reflection film preparation process and UV anti-reflection film are urgently needed to solve these problems. Summary of the invention
[0003] The purpose of the present application is to overcome the above technical problems and provide a preparation process of an ultraviolet anti-reflection film and an ultraviolet anti-reflection film.
[0004] In a first aspect, the present application provides a process for preparing an ultraviolet anti-reflection film, wherein the ultraviolet anti-reflection film comprises an anti-reflection film substrate, an aluminum oxide layer, and a silicon oxide layer from top to bottom; the preparation process comprises the following steps: S1. Wipe the surface of the antireflection film substrate to make it clean, clean it, put it into the furnace for vacuum, and heat it to 300℃, keep the constant temperature for 40-60min, and then plate the film at 300℃. The first film layer is an aluminum oxide layer, and the evaporation rate is 5-8i / s. The ion source is used throughout the process, and the ion source energy is 600×300; S2, the second film layer is a silicon oxide layer, the evaporation rate is 8-12i / s, the ion source is used throughout the process, and the ion source energy is 600×300; S3, after the film layer is plated, annealing treatment is performed to obtain the ultraviolet anti-reflection film.
[0005] By adopting the above technical scheme, the preparation process of a UV anti-reflection film and the UV anti-reflection film proposed in this application are intended to fundamentally solve the problems of easy damage, low transmittance and poor thermal stability of traditional UV anti-reflection films. The process first deeply cleans and pre-treats the anti-reflection film substrate to ensure the cleanliness of the film attachment surface, and then, in a strictly controlled vacuum environment, by accurately adjusting the evaporation rate and ion source energy, the aluminum oxide layer and the silicon oxide layer are plated step by step to form a top-down multilayer structure. Specifically, in step S1, the aluminum oxide layer is first plated at a rate of 5-8i / s at 300°C. The aluminum oxide layer is used as the bottom layer. Due to its high hardness and excellent mechanical strength, it significantly improves the wear resistance and impact resistance of the film layer. Step S2 follows immediately, and the silicon oxide layer is plated at a rate of 8-12i / s. Due to its high thermal stability and excellent chemical stability, it can effectively enhance the overall high temperature resistance and resistance to external environmental erosion of the film layer. At the same time, the aluminum oxide layer also has good ultraviolet light transmittance characteristics, which further improves the optical properties of the film layer. The ion source was used throughout the process and the ion source energy was set to 600×300. The precise control of this parameter ensured the density and uniformity of the film layer, avoided the common microcracks and pores in the traditional preparation process, and enhanced the integrity and durability of the film layer. Finally, the annealing treatment in step S3 further optimized the microstructure of the film layer, promoted the bonding force between the layers of materials, and significantly improved the overall mechanical properties and thermal stability of the film layer. In summary, the UV anti-reflection film preparation process proposed in this application effectively solves the technical difficulties existing in traditional UV anti-reflection films through fine material selection, reasonable layered structure design and strict control of preparation conditions, significantly improves the durability, transmittance and thermal stability of the film layer, and provides a more reliable and efficient solution for applications in the field of ultraviolet light.
[0006] Optionally, the cleaning in step S1 is as follows: The substrate was cleaned using an ion source for 4-8 minutes, and the ion source energy was 600×300.
[0007] By adopting the above technical solution, the substrate is cleaned by an ion source for 4-8 minutes, and the ion source energy is set to 600×300, which can significantly improve the preparation quality and performance of the UV anti-reflection film. Before the film is plated, the substrate is deeply cleaned by the ion source, and the surface of the substrate is bombarded with high-energy ions to effectively remove the attached dust and pollutants, which not only greatly improves the cleanliness of the substrate, but also promotes the bonding strength between the subsequent film layer and the substrate. Specifically, the 600×300 ion source energy can generate a sufficiently strong ion flow to penetrate into the tiny pores on the surface of the substrate, remove impurities that are difficult to reach, and ensure high purity during the film coating process. At the same time, the appropriate cleaning time (4-8 minutes) can fully achieve the cleaning effect and avoid the damage to the substrate surface that may be caused by too long cleaning time. Through this pretreatment step, not only the defect rate in the film layer, such as microcracks and pores, is significantly reduced, but also the uniformity and density of the film layer are effectively improved, thereby greatly enhancing the durability, transmittance and thermal stability of the UV anti-reflection film. In short, this technical solution lays a solid foundation for the high-performance preparation of UV anti-reflection films through refined control of ion source cleaning parameters, providing more reliable and efficient optical components for UV light applications.
[0008] Optionally, the furnace vacuuming in step S1 is as follows: vacuuming to 5.0×10 -3 -6.0×10 -3 .
[0009] Optionally, the annealing process in step S3 is as follows: The temperature of the first stage is 20-30℃ and the time is 5-15 minutes; The second stage temperature is 45-55°C and the time is 5-15 minutes; The temperature of the third stage is 65-75°C and the time is 25-35 minutes.
[0010] By adopting the above technical solution, a staged temperature-increasing annealing treatment scheme is adopted, that is, the temperature in the first stage is 20-30℃ for 5-15 minutes, the temperature in the second stage is raised to 45-55℃ and also lasts for 5-15 minutes, and finally in the third stage the temperature is raised to 65-75℃ and maintained for 25-35 minutes. This technical solution is aimed at the preparation of ultraviolet anti-reflection film, which can significantly optimize the microstructure of the film layer and improve its comprehensive performance. After the film layer is plated, the annealing process with gradually increasing temperature can effectively relieve the residual stress inside the film layer, promote the rearrangement of the molecules in the film layer material, and enhance the density and bonding force of the film layer. Specifically, the initial low-temperature annealing (20-30°C, 5-15 minutes) helps to initially stabilize the film structure and prevent damage to the film caused by temperature changes; the subsequent medium-temperature annealing (45-55°C, 5-15 minutes) further consolidates the structural integrity of the film and reduces minor defects; the final high-temperature annealing (65-75°C, 25-35 minutes) is a key step, which can significantly increase the density of the film, reduce the internal porosity, and enhance the thermal stability and mechanical strength of the film, reducing the risk of contamination and damage that may be encountered in future use. Through this series of carefully designed annealing treatments, the common technical problems of high film stress, unstable structure, and poor durability in the preparation of traditional UV anti-reflection films have been effectively solved, and the optical performance and service life of the film have been significantly improved, providing strong support for technological innovation in the field of UV light applications.
[0011] Optionally, the transparent membrane substrate is selected from a quartz glass material substrate.
[0012] By adopting the above technical solution, the present application selects quartz glass as the material of the transparent film substrate, and this technical solution has significant advantages in the preparation of the ultraviolet anti-reflection film. Quartz glass has become an ideal substrate material in the field of ultraviolet light applications with its excellent optical properties and physical properties. First, quartz glass has extremely high ultraviolet light transmittance, especially in the deep ultraviolet region, its transmittance is far higher than other common materials, which directly improves the overall optical performance of the ultraviolet anti-reflection film, so that the film layer can transmit ultraviolet light more effectively and meet the needs of high-precision optical systems. Secondly, quartz glass has excellent thermal stability, can maintain structural stability under high temperature environment, and is not easy to deform, which is very important for the film coating and annealing treatment that needs to be carried out under high temperature conditions, ensuring the dimensional stability and film quality during the film preparation process. Furthermore, quartz glass has high chemical stability, can resist the erosion of various chemical substances, and can maintain good performance even in harsh working environments, extending the service life of the ultraviolet anti-reflection film. In addition, the low thermal expansion coefficient of quartz glass is also a major advantage, which can effectively reduce the film stress caused by temperature changes, and further improve the durability and reliability of the film layer. In summary, by choosing quartz glass as the transparent film substrate, not only the transmittance and thermal stability of the UV anti-reflection film are significantly enhanced, but also its chemical stability and durability are improved, providing higher quality optical components for UV light applications and promoting innovation and development in related technical fields.
[0013] Optionally, the thickness of the silicon oxide layer is 400-500 nm.
[0014] Preferably, the thickness of the silicon oxide layer is 436 nm.
[0015] By adopting the above technical solution, the thickness of the silicon oxide layer is set to 436nm, which plays a vital role in the preparation of the UV anti-reflection film. As a key component of the UV anti-reflection film, the precise control of the thickness of the silicon oxide layer directly affects the overall optical performance and durability of the film. The selection of the thickness of 436nm is based on the in-depth understanding and application of the principle of optical interference, aiming to achieve the maximum transmittance of ultraviolet light of a specific wavelength. Specifically, when the thickness of the silicon oxide layer matches the wavelength of the incident ultraviolet light, the optical interference effect can be effectively utilized to reduce the reflection loss of light on the surface of the film layer and significantly improve the transmittance of light. In addition, the thickness of 436nm also takes into account the mechanical strength and thermal stability of the film layer, ensuring that the film layer can maintain the structural integrity and functional stability when facing ultraviolet rays or laser impact, and is not prone to microcracks or falling off. More importantly, this thickness design also takes into account the durability and cost-effectiveness of the film layer, which not only ensures the optimization of the film layer performance, but also avoids unnecessary material waste, achieving a balance between high performance and economy. In short, by precisely setting the thickness of the silicon oxide layer to 436nm, not only the optical performance of the UV anti-reflection film is significantly improved, but also its durability and economy are enhanced, providing a more efficient, stable and cost-controlled optical solution for UV light applications.
[0016] Optionally, the thickness of the aluminum oxide layer is 600-800nm.
[0017] Preferably, the thickness of the aluminum oxide layer is 662 nm.
[0018] By adopting the above technical solution, the thickness of the aluminum oxide layer is set to 662nm, which plays a key role in the preparation of the ultraviolet anti-reflection film. As an important component of the film structure, the precise control of the thickness of the aluminum oxide layer is crucial to optimizing the optical properties of the film and improving its durability. The selection of the thickness of 662nm is based on a deep understanding of the characteristics of the aluminum oxide material and precise calculation of the film design, aiming to achieve efficient transmission of ultraviolet light and enhance the protective performance of the film. Specifically, the aluminum oxide layer has a high refractive index and good chemical stability, which can provide additional optical gain in the ultraviolet spectrum. At the same time, its high hardness can effectively resist external physical damage and protect the underlying aluminum oxide layer from wear. The thickness design of 662nm makes full use of these characteristics of the aluminum oxide layer, which not only ensures the high transmittance of ultraviolet light, but also significantly enhances the overall mechanical strength and damage resistance of the film, especially the stability of the film under long-term exposure to ultraviolet light. In addition, this thickness also takes into account the thermal stability of the film, which can maintain the integrity of the structure and the stability of the function in a high temperature environment, avoiding performance degradation caused by temperature changes. In summary, by setting the thickness of the aluminum oxide layer to 662nm, not only the optical performance of the UV anti-reflection film is significantly optimized, but also its durability and reliability in complex environments are greatly improved, providing high-performance and high-stability optical components for UV light applications and promoting the continuous advancement of related technologies.
[0019] Optionally, the refractive index of the silicon oxide at 300° C. is between 1.45 and 1.55; the refractive index of the aluminum oxide at 300° C. is between 1.62 and 1.75.
[0020] By adopting the above technical solution, by controlling the refractive index of silicon oxide at 300°C between 1.45-1.55 and the refractive index of aluminum oxide at the same temperature within the range of 1.62-1.75, this technical solution achieves significant optimization of optical performance in the preparation of ultraviolet anti-reflection film. The refractive index is one of the important parameters that determine the optical properties of the film layer. Especially in the multilayer film structure, the difference in the refractive index of different material layers directly affects the reflection and transmission effect of the film layer on light of a specific wavelength. At the specific temperature of 300°C, the refractive index of silicon oxide and aluminum oxide is in the range of 1.45-1.55 and 1.62-1.75, respectively, which can ensure the formation of effective optical interference between the two material layers, thereby achieving effective management of ultraviolet light. Specifically, the low refractive index of the silicon oxide layer combined with the high refractive index of the aluminum oxide layer can significantly reduce the reflection loss of light on the surface of the film layer and improve the transmittance of ultraviolet light. At the same time, this careful matching of the refractive index can also enhance the anti-reflection performance of the film layer, reduce the multiple reflections of light inside the film layer, and further improve the transmission efficiency of light. In addition, by precisely controlling the refractive index of the two materials at 300°C, the thermal stability of the film during the preparation process can be ensured, and the fluctuation of the refractive index caused by temperature changes can be avoided, thereby ensuring the consistency and reliability of the film performance. In summary, by controlling the refractive index of silicon oxide and aluminum oxide at 300°C within the range of 1.45-1.55 and 1.62-1.75, respectively, not only the optical performance of the UV anti-reflection film is optimized, but also its thermal stability and reliability are improved, providing high-performance and high-stability optical components for UV light applications, meeting the needs of modern optical systems for high-precision and high-efficiency UV light management.
[0021] In a second aspect, the present application provides an ultraviolet anti-reflection film, which is prepared by the preparation process provided by the present application.
[0022] By adopting the above technical scheme, a UV anti-reflection film provided by the present application is carefully crafted based on the innovative preparation process detailed above. The outstanding features of the UV anti-reflection film are its excellent optical properties, enhanced durability and excellent thermal stability, which are achieved by precisely controlling material selection, layer thickness, refractive index and preparation conditions. Specifically, the UV anti-reflection film uses quartz glass as a substrate to ensure its high transmittance and chemical stability within the ultraviolet spectrum. The multilayer structure design of the silicon oxide layer and the aluminum oxide layer combines the advantages of both in refractive index, hardness and chemical stability, and realizes efficient transmission of ultraviolet light and comprehensive protection of the film layer. Among them, the thickness of the silicon oxide layer is 436nm, and the refractive index is controlled between 1.45-1.55, while the thickness of the aluminum oxide layer is set to 662nm, and the refractive index is maintained in the range of 1.62-1.75. This precise parameter setting ensures that the film layer maximizes the utilization of ultraviolet light of a specific wavelength, while enhancing the mechanical strength and damage resistance of the film layer. In addition, the temperature control, ion source cleaning, and annealing treatment with increasing temperature in stages during the entire preparation process further optimize the microstructure of the film layer, improve the density and bonding strength of the film layer, reduce internal stress and defects, and thus significantly enhance the durability and thermal stability of the film layer. In particular, by plating and annealing the film layer at a temperature of 300°C, it not only promotes the bonding between the molecules of the film material, but also ensures that the film layer can withstand the test of high temperature environment in subsequent use, avoiding performance degradation caused by temperature changes. In summary, the ultraviolet anti-reflection film provided in this application, thanks to its innovative preparation process, not only performs well in terms of transmittance, durability and thermal stability, but also can adapt to various complex application environments, providing a solid foundation and unlimited possibilities for the wide application and future development of ultraviolet light technology.
[0023] In a third aspect, the present application provides an application of an ultraviolet anti-reflection film in photovoltaic glass and optical elements.
[0024] In summary, the present invention has at least the following beneficial effects: Since the present invention adopts the good bonding property of silicon oxide and aluminum oxide, the prepared ultraviolet antireflection film has a firm structure, is not easy to be damaged or fall off, and has a prolonged service life.
[0025] In the present invention, a specific film thickness and refractive index, as well as an annealing process are preferably used, so that the prepared ultraviolet anti-reflection film has the characteristics of high transmittance and resistance to long-term laser use, thereby improving the film performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 355nm band reflection spectrum data curve of the ultraviolet anti-reflection film prepared in Example 1; Figure 2This is the 355nm band reflection spectrum data curve of the ultraviolet anti-reflection film prepared in Comparative Example 1. DETAILED DESCRIPTION
[0027] The present application is further described below with reference to the accompanying drawings: Embodiment 1-7 provides a UV anti-reflection film. Example 1
[0028] This embodiment discloses an ultraviolet anti-reflection film, which comprises an anti-reflection film substrate, an aluminum oxide layer, and a silicon oxide layer from top to bottom; the preparation process comprises the following steps: S1. Wipe the surface of the anti-reflection film substrate (5mm) to make it clean, clean it, put it into the furnace for vacuum, and heat it to 300℃, keep the constant temperature for 50min, and then coat the film at 300℃. The first film layer is an aluminum oxide layer, and the evaporation rate is 6i / s. The ion source is used throughout the process, and the ion source energy is 600×300; S2, the second film layer is a silicon oxide layer, the evaporation rate is 10i / s, the ion source is used throughout the process, and the ion source energy is 600×300; S3. After the film layer is plated, an annealing treatment is performed to obtain an ultraviolet anti-reflection film.
[0029] The cleaning in step S1 is as follows: the substrate is cleaned for 6 minutes using an ion source with an ion source energy of 600×300.
[0030] The furnace is vacuumed in step S1 as follows: vacuumize to 6.0×10 -3 .
[0031] The annealing process in step S3 is as follows: The temperature of the first stage is 25°C and the duration is 10 minutes; The second stage temperature is 50°C and the time is 10 minutes; The temperature of the third stage is 70°C and the time is 30 minutes.
[0032] The transparent film substrate is selected from a quartz glass material substrate (with a thickness of 5 mm).
[0033] The thickness of the silicon oxide layer is 436 nm.
[0034] The thickness of the aluminum oxide layer is 662 nm.
[0035] The refractive index of silicon oxide at 300°C is between 1.45 and 1.55; The refractive index of aluminum oxide at 300°C is between 1.62 and 1.75. Example 2
[0036] The difference between this embodiment and embodiment 1 is that the preparation process includes the following steps: S1. Wipe the surface of the anti-reflection film substrate to make it clean, clean it, put it into the furnace for vacuum, and heat it to 300℃, keep the constant temperature for 40min, and then plate the film at 300℃. The first film layer is an aluminum oxide layer, and the evaporation rate is 4i / s. The ion source is used throughout the process, and the ion source energy is 600×300; S2, the second film layer is a silicon oxide layer, the evaporation rate is 8i / s, the ion source is used throughout the process, and the ion source energy is 600×300; S3. After the film layer is plated, an annealing treatment is performed to obtain an ultraviolet anti-reflection film.
[0037] The cleaning in step S1 is as follows: the substrate is cleaned for 4 minutes using an ion source with an ion source energy of 600×300. The rest is the same as in Example 1. Example 3
[0038] The difference between this embodiment and embodiment 1 is that the preparation process includes the following steps: S1. Wipe the surface of the anti-reflection film substrate to make it clean, clean it, put it into the furnace for vacuum, and heat it to 300℃, keep the constant temperature for 80min, and then plate the film at 300℃. The first film layer is an aluminum oxide layer, and the evaporation rate is 8i / s. The ion source is used throughout the process, and the ion source energy is 600×300; S2, the second film layer is a silicon oxide layer, the evaporation rate is 12i / s, the ion source is used throughout the process, and the ion source energy is 600×300; S3. After the film layer is plated, an annealing treatment is performed to obtain an ultraviolet anti-reflection film.
[0039] The cleaning in step S1 is as follows: the substrate is cleaned for 4 minutes using an ion source with an ion source energy of 600×300. The rest is the same as in Example 1. Example 4
[0040] The difference between this embodiment and embodiment 1 is that the annealing process in step S3 of this embodiment is as follows: The temperature of the first stage is 20°C and the duration is 15 minutes; The second stage temperature is 45°C and the time is 15 minutes; The temperature of the third stage is 65°C and the time is 35 minutes. Example 5
[0041] The difference between this embodiment and embodiment 1 is that the annealing process in step S3 of this embodiment is as follows: The temperature of the first stage is 30°C and the time is 5 minutes; The second stage temperature is 55°C and the time is 5 minutes; The temperature of the third stage is 75°C and the time is 25 minutes. Example 6
[0042] The difference between this embodiment and embodiment 1 is that in the ultraviolet antireflection film in this embodiment, the thickness of the silicon oxide layer is 400 nm, and the thickness of the aluminum oxide layer is 800 nm. Example 7
[0043] The difference between this embodiment and embodiment 1 is that in the ultraviolet antireflection film in this embodiment, the thickness of the silicon oxide layer is 500 nm and the thickness of the aluminum oxide layer is 600 nm. Comparative Example 1
[0044] The difference between this comparative example and Example 1 is that a single layer of magnesium fluoride in the prior art is used to plate an ultraviolet anti-reflection film. The following steps are included: the ultraviolet anti-reflection film in this comparative example is an anti-reflection film substrate and a magnesium fluoride layer from top to bottom; the preparation process includes the following steps: S1. Wipe the surface of the antireflection film substrate to make it clean, clean it, install it in a furnace to evacuate it, and heat it to 300℃, keep the constant temperature for 50 minutes, and then plate the film at 300℃. The first film layer is a magnesium fluoride layer. The evaporation rate is 10i / s. The ion source is used throughout the process, and the ion source energy is 600×300; S2. After the film layer is plated, an annealing treatment is performed to obtain an ultraviolet anti-reflection film.
[0045] The cleaning in step S1 is as follows: the substrate is cleaned for 6 minutes using an ion source with an ion source energy of 600×300.
[0046] The furnace is vacuumed in step S1 as follows: vacuumize to 6.0×10 -3 .
[0047] The annealing process in step S3 is as follows: The temperature of the first stage is 25°C and the duration is 10 minutes; The second stage temperature is 50°C and the time is 10 minutes; The temperature of the third stage is 70°C and the time is 30 minutes.
[0048] The transparent film substrate is selected from a quartz glass material substrate.
[0049] The thickness of the magnesium fluoride layer was 436 nm. Experimental testing:
[0050] The UV antireflection films prepared in Examples 1-7 and Comparative Example 1 were tested as follows: The Belarus RT spectrophotometer was used for index detection. Figure 1 (Example 1 UV anti-reflection film) It can be seen that the single-side reflectivity of the UV anti-reflection film prepared in Example 1 of the present application is 0.021%, the double-side transmittance is greater than 99.5%, and the laser damage threshold is increased from the original 3J / cm2 (Comparative Example 1) increased to 8J / cm 2 (laser pulse width 10ns), which increases the service life from the original 2 months to the current 8-12 months.
[0051] The single-side reflectivity of the UV antireflection film prepared in Example 2 is 0.025%, and the double-side transmittance is greater than 99.5%.
[0052] The single-side reflectivity of the UV antireflection film prepared in Example 3 is 0.023%, and the double-side transmittance is greater than 99.5%. Example 4
[0053] The single-side reflectivity of the UV antireflection film prepared in Example 4 is 0.026%, and the double-side transmittance is greater than 99.5%. Example 5
[0054] The single-side reflectivity of the UV antireflection film prepared in Example 5 is 0.032%, and the double-side transmittance is greater than 99.5%. Example 6
[0055] The single-side reflectivity of the UV antireflection film prepared in Example 6 is 0.028%, and the double-side transmittance is greater than 99.5%. Example 7
[0056] The single-side reflectivity of the UV antireflection film prepared in Example 7 is 0.030%, and the double-side transmittance is greater than 99.5%.
[0057] and, Figure 2 The 355nm band reflection spectrum data curve of the ultraviolet anti-reflection film prepared in Comparative Example 1 is shown in FIG. Figure 2 It can be seen that the single-side reflectivity of the UV anti-reflection film prepared in Comparative Example 1 is 1.692%.
[0058] It is not difficult to see that the UV anti-reflection film prepared in Examples 1-7 of the present application can achieve 355nm UV anti-reflection through film system design and process improvement, and reduces absorption and improves transmittance. The average transmittance is greater than 99.5%, and the single-sided reflection is less than 0.032%, which improves the anti-laser damage threshold and the service life.
[0059] In order to ensure the reliability of the optical element, environmental tests were carried out on the UV antireflection film samples prepared in Examples 1-7 and Comparative Example 1 according to the use requirements: Adhesion test: A 3M special tape with a width of 1 inch was placed close to the coating surface, and then quickly pulled up in the vertical direction of the film surface. After repeated pulling for 20 times, the UV anti-reflection films prepared in Examples 1 to 7 of the present application did not peel off. However, the UV anti-reflection film prepared in Comparative Example 1 peeled off after repeated pulling for 10 times.
[0060] Wet heat test: The UV anti-reflection films prepared in Examples 1-7 of the present application were immersed in water at a temperature of 50 degrees for 24 hours and there was no problem with the film layer.
[0061] However, the ultraviolet antireflection film prepared in Comparative Example 1 showed a film shedding phenomenon after being immersed in water at a temperature of 50 degrees for 24 hours.
[0062] High temperature resistance verification: The UV anti-reflection films prepared in Examples 1-7 of the present application were heated to 300 degrees at room temperature and baked for 2 hours and then cooled to room temperature, and there was no problem with the film layer.
[0063] However, the UV anti-reflection film prepared in Comparative Example 1 fell off after the temperature was raised to 300 degrees at room temperature and baked for 2 hours and then dropped to room temperature.
[0064] In summary, the UV anti-reflection films prepared in Examples 1 to 7 show significant advantages in optical properties, environmental adaptability and durability, which are specifically reflected in the following aspects compared with the UV anti-reflection film prepared in Comparative Example 1: The UV anti-reflection films of Examples 1 to 7 achieve extremely low single-sided reflectivity (less than 0.032%) and significantly improve the double-sided transmittance in the 355nm band (greater than 99.5%).
[0065] In addition, the improvement of the anti-laser damage threshold (from 3J / cm² to 8J / cm²) further enhances the ability of the film layer to resist high-energy density laser impact and extends the service life (from 1 month to 8-12 months). Through adhesion testing, wet heat testing and high temperature resistance verification, it is confirmed that the UV anti-reflection films prepared in Examples 1 to 7 can still maintain good stability in extreme environments, without problems such as film peeling, film shedding or falling. This shows that these film layers can withstand harsh conditions such as tape pulling, long-term immersion in hot water, and high-temperature baking, ensuring long-term reliability and safety. The reason why the UV anti-reflection films of Examples 1 to 7 have achieved significant breakthroughs in performance is due to the innovation of the film system design and the optimization of the process flow. The UV anti-reflection film provided in this application not only effectively reduces the reflection and absorption of light, but also greatly improves the transmittance, meeting the demand for efficient transmission of ultraviolet light in high-power laser systems. In summary, the UV anti-reflection films prepared in Examples 1 to 7 show excellent performance in terms of optical properties, environmental adaptability and durability. Compared with the UV anti-reflection film prepared in Comparative Example 1, they have obvious advantages both from the perspective of theoretical data and practical application, and provide a more reliable and efficient solution for UV light transmission in high-power laser systems.
[0066] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereby. Any equivalent replacement or improvement based on the technical solution of the present application shall be included in the protection scope of the present application.
Claims
1. A process for preparing an ultraviolet anti-reflection film, It is characterized in that The ultraviolet anti-reflection film comprises an anti-reflection film substrate, an aluminum oxide layer, and a silicon oxide layer from top to bottom; the preparation process comprises the following steps: S1. Wipe the surface of the antireflection film substrate to make it clean, clean it, put it into the furnace for vacuum, and heat it to 300℃, keep the constant temperature for 40-60min, and then plate the film at 300℃. The first film layer is an aluminum oxide layer, and the evaporation rate is 5-8i / s. The ion source is used throughout the process, and the ion source energy is 600×300; S2, the second film layer is a silicon oxide layer, the evaporation rate is 8-12i / s, the ion source is used throughout the process, and the ion source energy is 600×300; S3, after the film layer is plated, annealing treatment is performed to obtain the ultraviolet anti-reflection film.
2. The process for preparing the ultraviolet anti-reflection film according to claim 1, It is characterized in that The cleaning in step S1 is as follows: The substrate was cleaned using an ion source for 4-8 minutes, and the ion source energy was 600×300.
3. The preparation process of the ultraviolet anti-reflection film according to claim 1, It is characterized in that The furnace vacuuming in step S1 is as follows: vacuuming to 5.0×10 -3 -6.0×10 -3 .
4. The preparation process of the ultraviolet anti-reflection film according to claim 1, It is characterized in that The annealing process in step S3 is as follows: The temperature of the first stage is 20-30℃ and the time is 5-15 minutes; The second stage temperature is 45-55°C and the time is 5-15 minutes; The temperature of the third stage is 65-75°C and the time is 25-35 minutes.
5. The preparation process of the ultraviolet anti-reflection film according to claim 1, It is characterized in that The transparent membrane substrate is selected from a quartz glass material substrate.
6. The process for preparing the ultraviolet antireflection film according to claim 1, It is characterized in that The thickness of the silicon oxide layer is 400-500 nm.
7. The process for preparing the ultraviolet anti-reflection film according to claim 1, It is characterized in that The thickness of the aluminum oxide layer is 600-800nm.
8. The process for preparing the ultraviolet anti-reflection film according to claim 1, It is characterized in that The refractive index of the silicon oxide at 300° C. is between 1.45 and 1.55; the refractive index of the aluminum oxide at 300° C. is between 1.62 and 1.
75.
9. A UV anti-reflection film, It is characterized in that The invention is prepared by the preparation process according to any one of claims 1 to 8.
10. Use of the ultraviolet anti-reflection film according to claim 9 in photovoltaic glass and optical elements.