Method for forming protective film, protective film and semiconductor process equipment
By depositing a second protective film with higher density and smoothness on the inner wall of the process chamber, the problem of particulate contamination of the protective film under plasma bombardment was solved, thereby achieving uniformity of the impedance environment of the process chamber and improvement of wafer processing quality.
Patent Information
- Application Number
- CN202410969786.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
In existing technologies, protective films are prone to particulate contamination under plasma bombardment, and the impedance environment uniformity of the process chamber cannot be guaranteed, affecting wafer processing quality.
A first protective film is deposited on the inner wall of the process chamber, and a second protective film is deposited on its surface. The material of the second protective film is different from that of the first protective film, and it has higher density and smoothness. The deposition process is optimized by controlling the RF power supply and gas introduction parameters.
It effectively reduces the probability of particles forming on the protective film under plasma bombardment, improves the uniformity of plasma distribution in the process chamber, enhances the uniformity within and between wafers, and increases the wafer manufacturing capacity.
Smart Images

Figure CN118910591A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a method for forming a protective film, a protective film and semiconductor process equipment. Background Art
[0002] PECVD (Plasma Enhanced Chemical Vapor Deposition) is a chemical deposition system that uses glow discharge plasma to dissociate and recombine gaseous sources under low vacuum to achieve the growth of thin film materials. It has developed rapidly due to its advantages of fast deposition speed, low deposition temperature and support for the deposition of most dielectric films. In order to prevent metal contamination and particle contamination during the PECVD process and provide a stable impedance environment, a protective film is usually formed on the inner wall of the process chamber. However, during the current PECVD process, the protective film is very likely to produce particles under the bombardment of plasma, causing particle contamination, and the uniformity of the impedance environment of the process chamber cannot be guaranteed. Summary of the invention
[0003] In order to solve the above technical problems, the present invention discloses a method for forming a protective film, a protective film and semiconductor process equipment to solve the problem in the prior art that the protective film is easily contaminated by particles under the bombardment of plasma and the uniformity of the impedance environment of the process chamber cannot be guaranteed.
[0004] To achieve the above technical objectives, the embodiments of the present invention disclose the following technical solutions:
[0005] In a first aspect, an embodiment of the present invention discloses a method for forming a protective film, comprising: depositing a first protective film on the inner wall of a process chamber; depositing a second protective film on the surface of the first protective film; wherein the material of the second protective film is different from the material of the first protective film, and the density and smoothness of the second protective film are greater than the density and smoothness of the first protective film.
[0006] In one embodiment, the second protective film includes a nitrogen-doped silicon carbide film, and / or the first protective film includes a silicon oxide film.
[0007] In one embodiment, the thickness of the second protective film is smaller than the thickness of the first protective film.
[0008] In one embodiment, the thickness of the first protective film is greater than or equal to And / or, the thickness of the second protective film is less than or equal to
[0009] In one embodiment, when the first protective film is deposited on the inner wall of the process chamber, a first process gas is introduced into the process chamber, wherein the first process gas includes a first reaction gas and a second reaction gas, wherein the first reaction gas includes an oxygen-containing gas, and the second reaction gas includes a silicon-containing gas;
[0010] And / or, when depositing a second protective film on the surface of the first protective film, a second process gas is introduced into the process chamber, the second process gas includes a third reaction gas and a fourth reaction gas, the third reaction gas includes a nitrogen-containing gas, and the fourth reaction gas includes a carbon-silicon gas.
[0011] In one embodiment, when the duration of simultaneously introducing the first reaction gas and the second reaction gas into the process chamber reaches a first preset duration, controlling the first RF power source to start applying the first RF power to the interior of the process chamber;
[0012] And / or, when the duration for which the third reaction gas and the fourth reaction gas are simultaneously introduced into the process chamber reaches a second preset duration, the first RF power supply and the second RF power supply are controlled to be turned on to apply the second RF power and the third RF power to the interior of the process chamber respectively, and the frequency of the RF signal output by the first RF power supply is higher than the frequency of the RF signal output by the second RF power supply.
[0013] In one embodiment, after the deposition of the second protective film is completed and before the first RF power source and the second RF power source are turned off, the method further includes:
[0014] The first RF power source is controlled to apply a fourth RF power to the interior of the process chamber, wherein the fourth RF power is less than the second RF power.
[0015] In one embodiment, when the first process gas is introduced into the process chamber, the first reaction gas is introduced into the process chamber, and when a third preset time is reached, the second reaction gas is started to be introduced into the process chamber;
[0016] And / or, when the second process gas is introduced into the process chamber, the third reaction gas is introduced into the process chamber, and when a fourth preset time period is reached, the fourth reaction gas is started to be introduced into the process chamber.
[0017] In a second aspect, an embodiment of the present invention discloses a protective film, the protective film comprising a first protective film and a second protective film sequentially arranged in a thickness direction of an inner wall of a process chamber;
[0018] The material of the second protective film is different from that of the first protective film, and the density and smoothness of the second protective film are greater than those of the first protective film.
[0019] In one embodiment, the second protective film includes a nitrogen-doped silicon carbide film, and / or the first protective film includes a silicon oxide film.
[0020] In one embodiment, the thickness of the second protective film is smaller than the thickness of the first protective film.
[0021] In one embodiment, the thickness of the first protective film is greater than or equal to And / or, the thickness of the second protective film is less than or equal to
[0022] In the third aspect, an embodiment of the present invention discloses a semiconductor process equipment, comprising: a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller, the controller comprising at least one processor and at least one memory, the memory storing a computer program, and when the computer program is executed by the processor, the method for forming a protective film as described above is implemented.
[0023] In a fourth aspect, an embodiment of the present specification discloses a computer-readable storage medium, on which a computer program is stored. When the computer program is executed by a processor, the method for forming a protective film as described above is implemented.
[0024] In a fifth aspect, an embodiment of the present specification discloses a computer program product or a computer program, wherein the computer program product includes a computer program, and the computer program is stored in a computer-readable storage medium; the processor of the computer device reads the computer program from the computer-readable storage medium, and the processor implements the steps of the method for forming a protective film described above when executing the computer program.
[0025] The present invention discloses a method for forming a protective film, a protective film and a semiconductor process equipment. A first protective film is deposited on the inner wall of a process chamber, and a second protective film is deposited on the surface of the first protective film. The material of the second protective film is different from that of the first protective film, and the density of the second protective film is greater than that of the first protective film, so that the protective film has a stronger ability to resist plasma bombardment, thereby effectively reducing the probability of the protective film generating particles under the bombardment of plasma during the PECVD process, thereby reducing the risk of particle defects on the surface of the wafer; at the same time, the smoothness of the second protective film is greater than that of the first protective film, which effectively improves the uniformity of the impedance environment of the process chamber, thereby effectively ensuring the uniformity of the distribution of plasma in the process chamber during the PECVD process, and improving the uniformity within and between wafers. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the disclosed drawings without paying creative work.
[0027] Figure 1 A schematic flow chart of a method for forming a protective film disclosed in one embodiment of the present invention.
[0028] Figure 2 The present invention is a schematic flow chart of another method for forming a protective film disclosed in one embodiment of the present invention.
[0029] Figure 3 FIG. 4 is a schematic diagram showing a comparison of wet etching rates of a nitrogen-doped silicon carbide film deposited according to a method according to an embodiment of the present invention and a silicon oxide film deposited according to a conventional method.
[0030] Figure 4 This is the variation trend of the number of particles on the wafer with the cumulative film thickness of the process film.
[0031] Figure 5 The figure is a schematic diagram of the structure of a protective film disclosed in one embodiment of the present invention.
[0032] Figure 6 A schematic structural diagram of a semiconductor process equipment disclosed in one embodiment of the present invention. DETAILED DESCRIPTION
[0033] Unless otherwise defined, the technical terms or scientific terms used in the embodiments of this specification shall have the common meanings understood by persons with ordinary skills in the field to which this specification belongs. The words "first", "second" and similar words used in the embodiments of this specification do not indicate any order, quantity or importance, but are only used to avoid confusion of constituent elements.
[0034] Unless the context requires otherwise, throughout the specification, "plurality" means "at least two", and "including" is interpreted as an open, inclusive meaning, that is, "including, but not limited to". In the description of the specification, the terms "one embodiment", "some embodiments", "exemplary embodiments", "examples", "specific examples" or "some examples" are intended to indicate that a particular feature, structure, material or characteristic associated with the embodiment or example is included in at least one embodiment or example of the specification. The schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0035] The following will be combined with the drawings in the embodiments of this specification to clearly and completely describe the technical solutions in the embodiments of this specification. Obviously, the described embodiments are only part of the embodiments of this specification, not all of the embodiments. Based on the embodiments in this specification, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this specification.
[0036] At present, the performance improvement of computing and storage devices depends on the high integration of chip manufacturing. With the miniaturization of devices and the continuous increase of stacked film layers, higher requirements are placed on the repeatability, stability, defects and the control of the number of particles (in-film particles) in each process. However, the high-quality thin film deposition capability limits the throughput of wafer manufacturing to a certain extent, so higher requirements are placed on the process optimization of thin film deposition.
[0037] As mentioned in the background technology, PECVD (Plasma Enhanced Chemical Vapor Deposition) is a relatively mature chemical deposition system, which uses glow discharge plasma to dissociate and recombine gaseous sources under low vacuum to achieve the growth of thin film materials. PECVD has the advantages of fast deposition speed, low deposition temperature and supports the deposition of most dielectric films (such as the etch stop layer (ESL) of semiconductor devices, hard mask (HM), inter-metal dielectric layer (IMD) and inter-layer dielectric layer (ILD), etc.), so it has been rapidly developed and has a wide range of applications in the fields of ultra-large-scale integrated circuits, optoelectronic devices, MEMS (Micro-Electro-Mechanical System, micro-electromechanical system) and so on.
[0038] In order to prevent metal contamination and particle contamination during the PECVD process and provide a stable impedance environment, a protective film, i.e., a pre-coating layer, is usually formed on the inner wall of the process chamber to cover the metal inner wall of the process chamber through the protective film to prevent the metal inner wall from peeling off under the bombardment of plasma and causing metal contamination. At the same time, the protective film can be used as an intermediate adhesion layer to prevent the process film deposited during the PECVD process from peeling off on the inner wall of the process chamber and causing particle contamination; in addition, the protective film, as a dielectric layer, can balance the internal impedance of the process chamber to provide a stable impedance environment, thereby improving the stability of film deposition. For example, when the number of process films deposited in the process chamber reaches a predetermined number or the film thickness of the process film on the inner wall of the process chamber reaches a preset film thickness, a remote plasma (RPS) cleaning is performed to remove the accumulated film on the inner wall of the chamber, and a protective film is deposited on the inner wall of the process chamber before the next film deposition.
[0039] At present, in the process of depositing a protective film on the inner wall of the process chamber, usually only one layer of film is deposited, such as silicon oxide (SiO2) film. Silicon oxide is a common pre-coating material. As a commonly used dielectric layer, the process preparation method is mature, its uniformity is relatively easy to control, and it has good adhesion to the inner wall of the aluminum process chamber. At the same time, the PECVD method can obtain a thicker silicon oxide film in a shorter time, which is conducive to improving the equipment production capacity. However, the density of the silicon oxide film is low. During the PECVD process, especially in the high-power deposition process, it is very easy to be bombarded by plasma to produce particles, causing particle contamination. In addition, the unevenness and roughness of the silicon oxide film surface will affect the uniformity of the impedance environment in the process chamber, and thus the uniformity within and between wafers cannot be guaranteed during the PECVD process.
[0040] In addition, although the prior art can improve the density of the silicon oxide film to a certain extent by adjusting the process parameters during the silicon oxide film deposition process, thereby reducing the particle contamination during the PECVD process, it still cannot meet the requirements for wafer processing quality.
[0041] Therefore, it is necessary to disclose a method for forming a protective film to effectively reduce the risk of particle contamination of the protective film under plasma bombardment and improve the uniformity of the impedance environment of the process chamber.
[0042] In order to solve the problem that the protective film of the traditional method is very easy to cause particle contamination under the bombardment of plasma, and the uniformity of the impedance environment of the process chamber cannot be guaranteed, in the technical solution of the present invention, a first protective film is deposited on the inner wall of the process chamber, and a second protective film is deposited on the surface of the first protective film. The material of the second protective film is different from that of the first protective film, and the density of the second protective film is greater than that of the first protective film, so that the protective film has a stronger ability to resist plasma bombardment, thereby effectively reducing the probability of the protective film generating particles under the bombardment of plasma during the PECVD process, thereby reducing the risk of particle defects on the wafer surface; at the same time, the smoothness of the second protective film is greater than the smoothness of the first protective film, which effectively improves the uniformity of the impedance environment of the process chamber, and then during the PECVD process, it can effectively ensure the uniformity of the plasma distribution in the process chamber, and improve the uniformity within and between wafers.
[0043] In addition, the method for forming a protective film disclosed in the embodiment of the present invention also improves the process parameters during the deposition of the first protective film and the second protective film.
[0044] As an optional implementation of the disclosure of the present invention, an embodiment of the present invention discloses a method for forming a protective film, such as Figure 1 As shown, including:
[0045] S101 , depositing a first protective film on the inner wall of a process chamber.
[0046] Specifically, the process chamber can be a chamber for performing PECVD process processing, and the PECVD process processing includes but is not limited to the deposition of silicon oxide doped dielectric films, silicon carbide doped dielectric films, silicon nitride doped dielectric films, and silicon-based low dielectric constant (Low-K) dielectric films.
[0047] The inner wall of the process chamber may include every inner wall of the process chamber. The material of the first protective film may be a material with good adhesion to the inner wall of the process chamber to reduce the risk of the first protective film peeling off during the PECVD process. For example, the first protective film may include a silicon oxide film.
[0048] During the process of depositing the first protective film on the inner wall of the process chamber, the first process gas can be introduced into the process chamber, and the first target RF power supply can be controlled to turn on to deposit the first protective film. When the deposition of the first protective film is completed, the first target RF power supply can be turned off, and the introduction of the first process gas into the process chamber can be stopped, and the process chamber can be evacuated. The first process gas can include a reaction gas for reacting to obtain the first protective film, and can also include an inert gas. The first target RF power supply can include a first RF power supply, and can also include a first RF power supply and a second RF power supply at the same time. The frequency of the RF signal output by the first RF power supply can be higher than the frequency of the RF signal output by the second RF power supply. For example, the first RF power supply can be a high-frequency RF power supply, and the second RF power supply can be a low-frequency RF power supply.
[0049] S102, depositing a second protective film on the surface of the first protective film; wherein the material of the second protective film is different from that of the first protective film, and the density and smoothness of the second protective film are greater than those of the first protective film.
[0050] Specifically, when the deposition of the first protective film is completed, the second protective film can be further deposited on the surface of the first protective film, that is, the second protective film is adhered to the inner wall of the process chamber through the first protective film, and the pre-coated layer includes the first protective film and the second protective film. During the PECVD process in the process chamber, the surface of the second protective film can be in direct contact with the internal environment of the process chamber.
[0051] The material of the second protective film may be different from that of the first protective film. It should be noted that the material of the second protective film may have good adhesion to the first protective film to reduce the risk of peeling off between the first and second protective films during the PECVD process.
[0052] During the process of depositing the second protective film on the surface of the first protective film, a second process gas can be introduced into the process chamber, and the second target RF power source can be controlled to turn on to deposit the second protective film. When the deposition of the second protective film is completed, the second target RF power source can be turned off, and the introduction of the second process gas into the process chamber is stopped, and the process chamber is evacuated. The second process gas may include a reaction gas for reacting to obtain the second protective film, and may also include an inert gas. The second target RF power source may include the first RF power source, and may also include the first RF power source and the second RF power source at the same time.
[0053] Among them, the density of the second protective film can be greater than the density of the first protective film, that is, the second protective film has a stronger ability to resist plasma bombardment than the first protective film. Therefore, during the PECVD process, the probability of the protective film generating particles under the bombardment of plasma can be effectively reduced, thereby reducing the risk of particle defects on the wafer surface.
[0054] At the same time, the smoothness of the second protective film can be greater than the smoothness of the first protective film, that is, the surface of the pre-coated layer on the inner wall of the chamber that contacts the internal environment of the process chamber is smoother, and the roughness and unevenness are effectively reduced, thereby effectively improving the uniformity of the impedance environment of the process chamber. Therefore, during the PECVD process, the uniformity of the plasma distribution in the process chamber can be effectively guaranteed, thereby improving the uniformity within and between wafers.
[0055] At present, the single-layer silicon oxide film deposited on the inner wall of the process chamber has poor adhesion to the process film such as the silicon carbide-doped dielectric film deposited during the PECVD process. Therefore, the process film deposited during the PECVD process is very easy to peel off on the inner wall of the process chamber and cause particle contamination. In order to avoid the process film peeling off on the inner wall of the process chamber and causing particle contamination, the cumulative film thickness of the process film during the RPS cleaning interval is usually reduced. The cumulative film thickness of the process film is the total thickness of the process film deposited on the inner wall of the process chamber between two adjacent RPS cleanings. As a result, the RPS cleaning frequency is greatly increased. Since each RPS cleaning requires shutdown, the increase in the RPS cleaning frequency leads to a significant increase in the shutdown maintenance time, and the wafer manufacturing capacity cannot be guaranteed. In order to reduce the RPS cleaning frequency of the process chamber, in one embodiment of the present specification, the second protective film includes a nitrogen-doped silicon carbide film, and / or the first protective film includes a silicon oxide film.
[0056] Specifically, the nitrogen-doped silicon carbide film has similar atomic composition and better stress matching as the process film deposited during the PECVD process, and the process film includes but is not limited to silicon oxide-doped dielectric film, silicon carbide-doped dielectric film, silicon nitride-doped dielectric film and silicon-based low dielectric constant (Low-K) dielectric film, etc., thereby enhancing the adhesion between the nitrogen-doped silicon carbide film and the process film deposited during the PECVD process.
[0057] At the same time, the nitrogen-doped silicon carbide film has good adhesion to the silicon oxide film, and the silicon oxide film has good adhesion to the metal inner wall of the process chamber. Therefore, through the synergistic effect of the nitrogen-doped silicon carbide film and the silicon oxide film, during the PECVD process, the process chamber can be free from particles generated by the peeling of the process film at a large cumulative film thickness, thereby effectively reducing the RPS cleaning frequency and improving the wafer manufacturing capacity.
[0058] In addition, nitrogen-doped silicon carbide film has better density and smoothness, thus having stronger resistance to plasma bombardment, and can effectively improve the uniformity of the impedance environment of the process chamber, thereby further reducing the risk of particle defects on the wafer surface and improving the uniformity of plasma distribution in the process chamber.
[0059] In some embodiments of the present invention, the thickness of the second protective film is smaller than the thickness of the first protective film.
[0060] Specifically, the thickness of the second protective film may be smaller than that of the first protective film. For example, the thickness of the first protective film may be greater than or equal to the first preset thickness, the thickness of the second protective film may be less than or equal to the second preset thickness, and the first preset thickness may be greater than the second preset thickness.
[0061] Among them, since the density and smoothness of the second protective film are greater than the density and smoothness of the first protective film, the deposition rate of the second protective film is lower than the deposition rate of the first protective film. By setting the thickness of the second protective film to be smaller than the thickness of the first protective film, the deposition time of the pre-coating layer on the inner wall of the process chamber can be effectively shortened.
[0062] At the same time, by setting the thickness of the first protective film to be greater than or equal to the first preset thickness, the total thickness of the pre-coated layer on the inner wall of the process chamber can be effectively guaranteed, so that during the PECVD process, the thicker pre-coated layer can effectively balance the impedance in the process chamber, thereby providing a stable impedance environment for the process chamber, improving the uniformity of plasma distribution, and further improving the stability of thin film deposition during the PECVD process.
[0063] Therefore, by setting the thickness of the second protective film to be smaller than the thickness of the first protective film, the stability of the impedance environment of the process chamber can be effectively improved while shortening the deposition time of the pre-coating layer on the inner wall of the process chamber.
[0064] In some embodiments of the present invention, the thickness of the first protective film is greater than or equal to and / or, the thickness of the second protective film is less than or equal to
[0065] Specifically, the thickness of the first protective film may be greater than or equal to The thicker first protective film can effectively balance the impedance in the process chamber, thereby providing a stable impedance environment for the process chamber, improving the uniformity of plasma distribution, and further improving the stability of thin film deposition during the PECVD process.
[0066] In addition, the thickness of the second protective film can be less than or equal to On the one hand, since the second protective film has good density and smoothness, it has stronger resistance to plasma bombardment and can effectively improve the uniformity of the impedance environment of the process chamber, thereby reducing the risk of particle defects on the wafer surface and improving the uniformity of plasma distribution in the process chamber. On the other hand, it can effectively shorten the deposition time of the second protective film, thereby improving the deposition efficiency of the pre-coating layer on the inner wall of the process chamber.
[0067] In some embodiments of the present invention, when a first protective film is deposited on the inner wall of a process chamber, a first process gas is introduced into the process chamber, the first process gas includes a first reaction gas and a second reaction gas, the first reaction gas includes an oxygen-containing gas, and the second reaction gas includes a silicon-containing gas; and / or, when a second protective film is deposited on the surface of the first protective film, a second process gas is introduced into the process chamber, the second process gas includes a third reaction gas and a fourth reaction gas, the third reaction gas includes a nitrogen-containing gas, and the fourth reaction gas includes a carbon-silicon gas.
[0068] Specifically, the first process gas may include a first reaction gas and a second reaction gas, and the first reaction gas and the second reaction gas may be used to react to generate a first protective film. For example, the first reaction gas may include an oxygen-containing gas, such as laughing gas (N2O, nitrous oxide), oxygen (O2), carbon dioxide (CO2), etc., and the second reaction gas may include a silicon-containing gas, such as silane (SiH4). Exemplarily, the first reaction gas may be laughing gas, which is easy to react with silane, and the by-products of the reaction are less, which can effectively ensure the stability of the components of the first protective film, thereby improving the film-forming quality of the first protective film.
[0069] In implementation, the process chamber may include an inlet assembly, and when the first protective film is deposited on the inner wall of the process chamber, the first process gas may be introduced into the process chamber through the inlet assembly, and the first reaction gas and the second reaction gas in the first process gas may react in a plasma state to achieve deposition of the first protective film. The gas flow rate of the first reaction gas may range from 100 to 30,000 sccm, and the gas flow rate of the second reaction gas may range from 100 to 5,000 sccm.
[0070] The second process gas may include a third reaction gas and a fourth reaction gas, and the third reaction gas and the fourth reaction gas may be used to react to form a second protective film. For example, the third reaction gas may include a nitrogen-containing gas, such as ammonia (NH3), and the fourth reaction gas may include a carbon silicon-based gas, such as tetramethylsilane (Si(CH3)4), trimethylsilane (C3H 10 For example, the fourth reaction gas may be tetramethylsilane, which is easy to react with ammonia and produces fewer byproducts, and can effectively ensure the stability of the components of the second protective film, thereby improving the film-forming quality of the second protective film.
[0071] In implementation, when the second protective film is deposited on the surface of the first protective film, the second process gas can be introduced into the process chamber through the gas inlet assembly, and the third reaction gas and the fourth reaction gas in the second process gas can react in a plasma state to achieve the deposition of the second protective film. The gas flow rate of the third reaction gas can range from 1000 to 10000 sccm, and the gas flow rate of the fourth reaction gas can range from 100 to 10000 sccm.
[0072] It is understandable that the first process gas and / or the second process gas may also include an inert gas, such as nitrogen (N2), helium (He), argon (Ar), etc. For example, the inert gas may be nitrogen. The inert gas does not react during the deposition of the first protective film and / or the second protective film, and by introducing the inert gas into the process chamber, the reactive gas in the first process gas and / or the reactive gas in the second process gas can be evenly distributed inside the process chamber, thereby effectively improving the uniformity of film formation.
[0073] When the first protective film is deposited on the inner wall of the process chamber, the gas flow rate of the inert gas may range from 1000 to 5000 sccm; when the second protective film is deposited on the surface of the first protective film, the gas flow rate of the inert gas may range from 1000 to 10000 sccm.
[0074] In order to further improve the deposition rate of the first protective film and the second protective film, in some embodiments of the present invention, when the time duration for simultaneously introducing the first reaction gas and the second reaction gas into the process chamber reaches a first preset time duration, the first RF power supply is controlled to be turned on to apply the first RF power to the interior of the process chamber; and / or, when the time duration for simultaneously introducing the third reaction gas and the fourth reaction gas into the process chamber reaches a second preset time duration, the first RF power supply and the second RF power supply are controlled to be turned on to apply the second RF power and the third RF power to the interior of the process chamber, respectively, and the frequency of the RF signal output by the first RF power supply is higher than the frequency of the RF signal output by the second RF power supply.
[0075] Specifically, during the process of depositing the first protective film on the inner wall of the process chamber, when the time duration for simultaneously introducing the first reaction gas and the second reaction gas into the process chamber reaches a first preset time duration, the first RF power supply can be controlled to turn on. By turning on the first RF power supply, a high-frequency RF field can be applied inside the process chamber to provide energy through the high-frequency RF field to excite the reaction gas corresponding to the first protective film to dissociate into gas molecules.
[0076] The first preset time may be in the range of 1 to 5 seconds, so as to ensure that the first reaction gas and the second reaction gas in the process chamber are evenly distributed before turning on the first RF power supply, thereby further improving the film formation uniformity of the first protective film.
[0077] During implementation, the RF power of the first RF power can be adjusted to the first RF power, and the first RF power can be determined based on the first target deposition rate of the first protective film. For example, for different reaction gases, the correspondence between the first RF power and the first target deposition rate can be set, and the first RF power of the first RF power can be determined according to the reaction gas corresponding to the first protective film and the first target deposition rate of the first protective film. Then, by controlling the first RF power to turn on and apply the first RF power to the inside of the process chamber, the deposition rate of the first protective film can be effectively accelerated.
[0078] In addition, during the process of depositing the second protective film on the first protective film, when the duration of simultaneously introducing the third reaction gas and the fourth reaction gas into the process chamber reaches a second preset duration, the first RF power supply and the second RF power supply can be controlled to be turned on at the same time, and the frequency of the RF signal output by the first RF power supply is higher than the frequency of the RF signal output by the second RF power supply. By turning on the first RF power supply, a high-frequency RF field can be applied inside the process chamber, so that the high-frequency RF field can provide energy to excite the reaction gas corresponding to the second protective film to dissociate into gas molecules. By turning on the second RF power supply, a low-frequency RF field can be applied inside the process chamber, so that the low-frequency RF field can provide energy to excite the dissociated gas molecules to recombine, thereby effectively improving the recombination probability of the dissociated gas molecules, thereby improving the film formation rate of the second protective film.
[0079] The second preset time may range from 1 to 60 seconds to ensure that the third reaction gas and the fourth reaction gas in the process chamber are evenly distributed before turning on the first RF power supply and the second RF power supply, thereby further improving the film formation uniformity of the second protective film.
[0080] During implementation, the RF power of the first RF power can be adjusted to the second RF power and the RF power of the second RF power can be adjusted to the third RF power. The second RF power and the third RF power can be determined based on the second target deposition rate of the second protective film. For example, for different reaction gases, the correspondence between the second RF power and the third RF power and the second target deposition rate can be set, and the second RF power of the first RF power and the third RF power of the second RF power can be determined according to the reaction gas corresponding to the second protective film and the second target deposition rate of the second protective film. Furthermore, by controlling the first RF power and the second RF power to turn on and applying the second RF power and the third RF power to the inside of the process chamber respectively, the deposition rate of the second protective film can be effectively accelerated.
[0081] It is understandable that a spray assembly and a wafer carrier can be arranged inside the process chamber, the spray assembly is used to evenly distribute the process gas entering the process chamber, and the first RF power supply and the second RF power supply can provide RF power through the spray assembly. The wafer carrier can be grounded, and when the first RF power supply and / or the second RF power supply are turned on, a bias voltage can also be generated between the spray assembly and the wafer carrier, and the bias voltage can effectively increase the mean free path of the gas molecules obtained by dissociation, further increasing the deposition rate of the first protective film and the second protective film.
[0082] In some embodiments of the present invention, after the deposition of the second protective film is completed and before the first RF power supply and the second RF power supply are turned off, it also includes: controlling the first RF power supply to apply a fourth RF power to the inside of the process chamber, and the fourth RF power is less than the second RF power.
[0083] Specifically, during the deposition process of the second protective film, the deposition time of the second protective film can be monitored in real time. The deposition time of the second protective film may include the turn-on time of the first RF power supply and / or the second RF power supply, and when the deposition time of the second protective film reaches a preset deposition time, it is determined that the deposition of the second protective film is completed.
[0084] When the second protective film deposition is completed, the output power of the first RF power supply can be adjusted. For example, the first RF power supply can be controlled to apply a fourth RF power to the inside of the process chamber. The fourth RF power can be less than the second RF power to reduce the output power of the first RF power supply.
[0085] By reducing the output power of the first RF power supply, the dissociation rate of the reaction gas corresponding to the second protective film can be effectively reduced, so that the gas molecules dissociated in the process chamber can be fully recombinated. At the same time, by continuously applying RF power to the inside of the process chamber through the first RF power supply, the gas molecules dissociated in the process chamber can be placed in a suspended state, thereby avoiding directly turning off the first RF power supply at the end of the deposition of the second protective film, causing the unrecombined gas molecules to fall and produce particles, thereby affecting the smoothness and density of the second protective film, thereby effectively improving the film formation quality of the second protective film.
[0086] It can be understood that after the deposition of the second protective film is completed and before the first RF power supply and the second RF power supply are turned off, the second RF power supply can also be controlled to apply a fifth RF power to the inside of the process chamber. The fifth RF power can be less than the third RF power to reduce the output power of the second RF power supply.
[0087] Before shutting down the first RF power supply and the second RF power supply, by reducing the output power of the first RF power supply and the second RF power supply, the RF field in the process chamber can be smoothly withdrawn, thereby effectively avoiding sudden changes in plasma conditions in the process chamber caused by directly shutting down the first RF power supply and the second RF power supply, such as temperature, stress, etc., thereby avoiding reduced density and cracks of the second protective film due to sudden changes in plasma conditions, thereby effectively ensuring the film formation quality of the second protective film.
[0088] In some embodiments of the present invention, the second radio frequency power ranges from 100 to 2000W, and / or the third radio frequency power ranges from 100 to 2000W.
[0089] Specifically, the second RF power may be in the range of 100 to 2000 W (including the endpoint values), and the third RF power may be in the range of 100 to 2000 W (including the endpoint values). In implementation, the second RF power and the third RF power may be determined based on the film quality requirements of the second protective film (e.g., the particle condition of the second protective film) and the film forming rate requirements.
[0090] It can be understood that the range of the fourth RF power can be the same as the range of the second RF power, and the fourth RF power is less than the second RF power; in addition, the range of the fifth RF power can be the same as the range of the third RF power, and the fifth RF power is less than the third RF power.
[0091] In addition, the first RF power may range from 100 to 2000 W (including endpoint values). In implementation, the first RF power may be determined based on the film quality requirements of the first protective film (eg, the particle condition of the first protective film).
[0092] In order to further improve the uniformity of the first protective film and / or the second protective film, in one embodiment of the present specification, when the first process gas is introduced into the process chamber, the first reaction gas is introduced into the process chamber, and when the third preset time is reached, the second reaction gas is introduced into the process chamber;
[0093] And / or, when the second process gas is introduced into the process chamber, the third reaction gas is introduced into the process chamber, and when a fourth preset time is reached, the fourth reaction gas starts to be introduced into the process chamber.
[0094] Specifically, when the first process gas is introduced into the process chamber, the first reaction gas and the inert gas may be introduced into the process chamber first, so that the first reaction gas is evenly distributed inside the process chamber. When the third preset time is reached, the second reaction gas begins to be introduced into the process chamber, that is, when the third preset time is reached, the first reaction gas, the inert gas, and the second reaction gas are introduced into the process chamber at the same time, thereby, by introducing the second reaction gas after the first reaction gas is evenly distributed inside the process chamber, the uniformity of the first protective film can be effectively ensured.
[0095] During implementation, during the process of depositing the first protective film on the inner wall of the process chamber, the first reaction gas and the inert gas can be first introduced into the process chamber. When the third preset time is reached, the second reaction gas is started to be introduced into the process chamber. When the time for introducing the second reaction gas reaches the first preset time, the first RF power supply is controlled to turn on to deposit the first protective film, thereby further improving the uniformity of the first protective film.
[0096] When the second process gas is introduced into the process chamber, the third reaction gas and the inert gas may be introduced into the process chamber first, so that the third reaction gas is evenly distributed inside the process chamber. When the fourth preset time is reached, the fourth reaction gas begins to be introduced into the process chamber, that is, when the fourth preset time is reached, the third reaction gas, the inert gas and the fourth reaction gas are introduced into the process chamber at the same time, thereby, by introducing the fourth reaction gas after the third reaction gas is evenly distributed inside the process chamber, the uniformity of the second protective film can be effectively ensured.
[0097] During implementation, during the process of depositing the second protective film on the surface of the first protective film, the third reaction gas and the inert gas can be first introduced into the process chamber. When the fourth preset time is reached, the fourth reaction gas is started to be introduced into the process chamber. When the time for introducing the fourth reaction gas reaches the second preset time, the first RF power supply and the second RF power supply are controlled to turn on to deposit the second protective film, thereby further improving the uniformity of the second protective film.
[0098] The following is an example of an implementation process of the method for forming a protective film of the present invention. Figure 2 As shown, including:
[0099] S201. Inert gas nitrogen and the first reaction gas nitrous oxide are introduced into the process chamber to mix and control the pressure before the first protective film is deposited. In this step, the gas flow rate of nitrogen is in the range of 1000 to 5000 sccm; the gas flow rate of nitrous oxide is in the range of 100 to 30000 sccm; the pressure control range is 0.1 to 10 torr; the execution time of this step is in the range of 1 to 60 seconds.
[0100] S202, introducing the second reaction gas silane into the process chamber to mix and control the pressure of all reaction gases including silane before the first protective film is deposited. In this step, the gas flow rate of silane is in the range of 100 to 5000 sccm; the gas flow rate of nitrogen is in the range of 1000 to 5000 sccm; the gas flow rate of nitrous oxide is in the range of 100 to 30000 sccm; the pressure control range is 0.1 to 10 torr; and the execution time of this step is in the range of 1 to 5 seconds.
[0101] S203, control the first RF power supply to turn on, apply the first RF power to the inside of the process chamber to deposit a first protective film on the inner wall of the process chamber; in this step, the range of the first RF power is 100-2000W; the range of the gas flow rate of silane is 100-5000sccm; the range of the gas flow rate of nitrogen is 1000-5000sccm; the range of the gas flow rate of nitrous oxide is 100-30000sccm; the range of pressure control is 0.1-10torr; the execution time of this step is in the range of 10-600sec.
[0102] S204, stop introducing the second reaction gas silane into the process chamber to stop the deposition of the first protective film; in this step, the gas flow rate of nitrogen, the gas flow rate of nitrous oxide and the first RF power remain unchanged compared to step S203, and only stop introducing the second reaction gas silane into the process chamber.
[0103] S205, controlling the first radio frequency power supply to be turned off, stopping the introduction of the inert gas nitrogen and the first reaction gas nitrous oxide into the process chamber, and controlling the process chamber to be evacuated.
[0104] S206. Inert gas nitrogen and third reaction gas ammonia are introduced into the process chamber to mix and control the pressure before the second protective film is deposited. In this step, the gas flow rate of nitrogen is in the range of 1000 to 10000 sccm; the gas flow rate of ammonia is in the range of 1000 to 10000 sccm; the pressure control range is 0.1 to 10 torr; the execution time of this step is in the range of 1 to 60 seconds.
[0105] S207. Introduce tetramethylsilane, a fourth reaction gas, into the process chamber to mix and control the pressure of all reaction gases including tetramethylsilane before the second protective film is deposited. In this step, the gas flow rate of tetramethylsilane ranges from 100 to 10,000 sccm; the gas flow rate of nitrogen ranges from 1,000 to 10,000 sccm; the gas flow rate of ammonia ranges from 1,000 to 10,000 sccm; the pressure control range is 0.1 to 10 torr; the execution time of this step ranges from 1 to 60 seconds.
[0106] S208, control the first RF power supply and the second RF power supply to turn on, and apply the second RF power and the third RF power to the inside of the process chamber respectively, so as to deposit a second protective film on the inner wall of the process chamber; in this step, the range of the second RF power is 100-2000W, and the range of the third RF power is 100-2000W; the range of the gas flow rate of tetramethylsilane is 100-10000sccm; the range of the gas flow rate of nitrogen is 1000-10000sccm; the range of the gas flow rate of ammonia is 1000-10000sccm; the range of pressure control is 0.1-10torr; the execution time of this step is in the range of 1-600sec.
[0107] S209, adjust the output power of the first RF power supply and the second RF power supply, and apply the fourth RF power and the fifth RF power to the inside of the process chamber respectively, so as to prepare before shutting down the first RF power supply and the second RF power supply: in this step, the range of the fourth RF power is 100-2000W, the range of the fifth RF power is 100-2000W, the fourth RF power is less than the second RF power, and the fifth RF power is less than the third RF power; the gas flow rate of tetramethylsilane is in the range of 100-10000sccm; the gas flow rate of nitrogen is in the range of 1000-10000sccm; the gas flow rate of ammonia is in the range of 1000-10000sccm; the pressure control range is 0.1-10torr; the execution time of this step ranges from 1 to 60sec.
[0108] S210, turning off the first RF power supply and the second RF power supply, stopping the introduction of the inert gas nitrogen, the third reaction gas ammonia and the fourth reaction gas tetramethylsilane into the process chamber, and controlling the process chamber to evacuate.
[0109] The beneficial effects of the method for forming a protective film in this embodiment are verified by experiments as follows.
[0110] Wet Etch Rate (WER) Verification: Four groups of samples were prepared, each group of samples including a nitrogen-doped silicon carbide film deposited on a bare silicon wafer according to the method of this embodiment, and a silicon oxide film deposited on a bare silicon wafer according to the existing method; the four groups of samples were wet etched in a 100:1 hydrofluoric acid solution, and the wet etching rate comparison of the nitrogen-doped silicon carbide film and the silicon oxide film can be shown as follows: Figure 3 As shown by Figure 3 It can be seen that the wet etching rate of the nitrogen-doped silicon carbide film is much lower than that of the silicon oxide film. It can be seen that the nitrogen-doped silicon carbide film deposited according to the method of this embodiment has higher density and etching resistance than the silicon oxide film deposited according to the existing method. Therefore, by depositing the nitrogen-doped silicon carbide film on the surface of the first protective film in the process chamber, the probability of the nitrogen-doped silicon carbide film generating particles under the bombardment of plasma can be effectively reduced, thereby reducing the risk of particle defects on the wafer surface.
[0111] Wafer particle contamination verification: Based on the method of this embodiment, a first protective film is deposited on the inner wall of the process chamber and a second protective film is deposited on the surface of the first protective film. When the PECVD process is performed in the process chamber, the cumulative film thickness of the process film is calculated. Growth to The number of particles larger than 0.4 μm on the wafer during the process can be statistically analyzed as follows: Figure 4 As shown. Figure 4 It can be seen that with the increase of the cumulative film thickness of the process film, the number of particles on the wafer has not increased significantly. It can be seen that the protective film prepared by the method of this embodiment has a good inhibitory effect on wafer particle contamination. The second protective film acts as an excellent intermediate adhesion layer between the first protective film and the process film. At the same time, it effectively increases the cumulative film thickness of the process film in the RPS cleaning interval, thereby improving the production capacity of wafer manufacturing.
[0112] As an optional implementation of the content disclosed in the present invention, the embodiment of the present invention further discloses a protective film, referring to Figure 5, the protective film 300 includes a first protective film 301 and a second protective film 302 sequentially arranged in the thickness direction of the inner wall of the process chamber 20; wherein, the material of the second protective film 302 is different from that of the first protective film 301, and the density and smoothness of the second protective film 302 are greater than those of the first protective film 301. That is, the second protective film 302 is adhered to the inner wall of the process chamber 20 through the first protective film 301. During the PECVD process in the process chamber 20, the surface of the second protective film 302 can be in direct contact with the internal environment of the process chamber 20. By setting the density of the second protective film 302 to be greater than that of the first protective film 301, the second protective film 302 has a stronger ability to resist plasma bombardment than the first protective film 301. Therefore, during the PECVD process, the probability of the protective film 300 generating particles under the bombardment of plasma can be effectively reduced, thereby reducing the risk of particle defects on the wafer surface. At the same time, by setting the smoothness of the second protective film 302 to be greater than the smoothness of the first protective film 301, the surface of the protective film 300 in contact with the internal environment of the process chamber 20 is smoother, and the roughness and unevenness are effectively reduced, thereby effectively improving the uniformity of the impedance environment of the process chamber 20. Therefore, during the PECVD process, the uniformity of the plasma distribution in the process chamber 20 can be effectively guaranteed, thereby improving the uniformity within the wafer and between wafers.
[0113] Exemplarily, the second protective film 302 includes a nitrogen-doped silicon carbide film, and / or the first protective film 301 includes a silicon oxide film, the nitrogen-doped silicon carbide film has an atomic composition similar to that of the process film deposited during the PECVD process and better stress matching, thereby enhancing the adhesion between the second protective film 302 and the process film deposited during the PECVD process. At the same time, the nitrogen-doped silicon carbide film has good adhesion to the silicon oxide film, and the silicon oxide film has good adhesion to the metal inner wall of the process chamber 20. Therefore, through the synergistic effect of the first protective film 301 and the second protective film 302, during the PECVD process, the process chamber 20 can be made to not produce particles caused by the peeling of the process film at a large cumulative film thickness, thereby effectively reducing the RPS cleaning frequency and improving the wafer manufacturing capacity. In addition, the nitrogen-doped silicon carbide film has better density and smoothness, thus having a stronger ability to resist plasma bombardment, and can effectively improve the uniformity of the impedance environment of the process chamber 20, thereby further reducing the risk of particle defects on the wafer surface and improving the uniformity of plasma distribution in the process chamber 20.
[0114] Exemplarily, the thickness of the second protective film 302 is less than that of the first protective film 301, which can effectively shorten the deposition time of the protective film 300 on the inner wall of the process chamber 20. At the same time, the overall thickness of the protective film 300 can be ensured, so that the protective film 300 can effectively balance the impedance in the process chamber 20, thereby providing a stable impedance environment for the process chamber 20, improving the uniformity of plasma distribution, and further improving the stability of thin film deposition during the PECVD process.
[0115] Exemplarily, the thickness of the first protective film 301 is greater than or equal to And / or, the thickness of the second protective film 302 is less than or equal to By setting a thicker first protective film 301, the impedance in the process chamber 20 can be effectively balanced, thereby providing a stable impedance environment for the process chamber 20, improving the uniformity of plasma distribution, and further improving the stability of thin film deposition during the PECVD process; at the same time, by setting a thinner second protective film 302, the deposition time of the second protective film 302 can be effectively shortened, thereby improving the deposition efficiency of the protective film 300 on the inner wall of the process chamber 20.
[0116] As an optional implementation of the content disclosed in the present invention, the embodiment of the present invention further discloses a semiconductor process equipment, referring to Figure 6 The semiconductor process equipment 200 includes a process chamber 20, an inlet assembly 20A, an upper electrode assembly 20B, a lower electrode assembly 20C and a controller ( Figure 6 The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method for forming a protective film in any of the above embodiments is implemented.
[0117] Exemplarily, the controller can be a host computer or a slave computer. The controller can control the valve of the air inlet component 20A to open so as to introduce the corresponding process gas into the interior of the process chamber 20; the controller can also control the opening and closing degree of the valve of the air inlet component 20A to control the flow rate of the process gas. The semiconductor process equipment 200 can also include a vacuum component 24, and the controller can control the vacuum degree inside the process chamber 20 by controlling the vacuum component 24. The semiconductor process equipment 200 can also include a heating component 25, and the controller can control the temperature inside the process chamber 20 by controlling the heating component 25 to heat the interior of the process chamber 20.
[0118] The upper electrode assembly 20B includes an RF power supply 21 and a spray assembly 22. The RF power supply 21 may include a first RF power supply and a second RF power supply. The first RF power supply may be a high-frequency RF power supply, and the second RF power supply may be a low-frequency RF power supply. The controller is also used to control the RF power supply 21 to provide the upper electrode power to the spray assembly 22 to excite the process gas inside the process chamber 20 to generate plasma 100. The upper electrode assembly 20B may also include a matcher 26. The RF power supply 21 may provide the upper electrode power to the spray assembly 22 through the matcher 26 to ensure the maximization of the RF power feed. The matcher 26 may include a first matcher and a second matcher. The first RF power supply and the second RF power supply provide the upper electrode power to the spray assembly 22 through the first matcher and the second matcher, respectively.
[0119] The lower electrode assembly 20C includes a wafer carrier 23 , which may be grounded. The wafer carrier 23 may be, for example, an electrostatic chuck, a mechanical chuck, or a vacuum adsorption chuck.
[0120] The semiconductor process equipment 200 disclosed in the embodiment of the present invention may be a high-density plasma chemical vapor deposition equipment or a plasma enhanced chemical vapor deposition equipment.
[0121] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0122] The above embodiments only express several implementation methods of this specification, and the descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the solutions disclosed in the embodiments of this specification. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of this specification, which all belong to the protection scope of this specification. Therefore, the protection scope of the patent of this specification shall be based on the attached claims.
Claims
1. A method for forming a protective film, characterized in that: include: Depositing a first protective film on an inner wall of the process chamber; A second protective film is deposited on the surface of the first protective film; wherein the material of the second protective film is different from that of the first protective film, and the density and smoothness of the second protective film are greater than those of the first protective film.
2. The method according to claim 1, characterized in that The second protection film includes a nitrogen-doped silicon carbide film, and / or the first protection film includes a silicon oxide film.
3. The method according to claim 1, characterized in that The thickness of the second protection film is smaller than the thickness of the first protection film.
4. The method according to claim 3, characterized in that The thickness of the first protective film is greater than or equal to And / or, the thickness of the second protective film is less than or equal to 5. The method according to claim 2, characterized in that: When depositing the first protective film on the inner wall of the process chamber, a first process gas is introduced into the process chamber, wherein the first process gas includes a first reaction gas and a second reaction gas, wherein the first reaction gas includes an oxygen-containing gas and the second reaction gas includes a silicon-containing gas; And / or, when depositing a second protective film on the surface of the first protective film, a second process gas is introduced into the process chamber, the second process gas includes a third reaction gas and a fourth reaction gas, the third reaction gas includes a nitrogen-containing gas, and the fourth reaction gas includes a carbon-silicon gas.
6. The method according to claim 5, characterized in that When the duration of simultaneously introducing the first reaction gas and the second reaction gas into the process chamber reaches a first preset duration, controlling the first radio frequency power source to start applying the first radio frequency power to the interior of the process chamber; And / or, when the duration for which the third reaction gas and the fourth reaction gas are simultaneously introduced into the process chamber reaches a second preset duration, the first RF power supply and the second RF power supply are controlled to be turned on to apply the second RF power and the third RF power to the interior of the process chamber respectively, and the frequency of the RF signal output by the first RF power supply is higher than the frequency of the RF signal output by the second RF power supply.
7. The method according to claim 6, characterized in that After the deposition of the second protective film is completed and before the first RF power source and the second RF power source are turned off, the method further includes: The first RF power source is controlled to apply a fourth RF power to the interior of the process chamber, wherein the fourth RF power is less than the second RF power.
8. The method according to any one of claims 5 to 7, characterized in that: When the first process gas is introduced into the process chamber, the first reaction gas is introduced into the process chamber, and when a third preset time is reached, the second reaction gas is started to be introduced into the process chamber; And / or, when the second process gas is introduced into the process chamber, the third reaction gas is introduced into the process chamber, and when a fourth preset time period is reached, the fourth reaction gas is started to be introduced into the process chamber.
9. A protective film, characterized in that: The protective film includes a first protective film and a second protective film sequentially arranged in a thickness direction of the inner wall of the process chamber; The material of the second protective film is different from that of the first protective film, and the density and smoothness of the second protective film are greater than those of the first protective film.
10. The protective film according to claim 9, characterized in that: The second protection film includes a nitrogen-doped silicon carbide film, and / or the first protection film includes a silicon oxide film.
11. The protective film according to claim 9, characterized in that: The thickness of the second protection film is smaller than the thickness of the first protection film.
12. The protective film according to claim 11, characterized in that: The thickness of the first protective film is greater than or equal to And / or, the thickness of the second protective film is less than or equal to 13. A semiconductor process equipment, characterized in that: include: A process chamber, an air inlet assembly, an upper electrode assembly, a lower electrode assembly and a controller, wherein the controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method for forming a protective film according to any one of claims 1 to 8 is implemented.
Citation Information
Patent Citations
Method for pre-depositing high-density plasma machine platform
CN102586758A
Method for depositing amorphous silicon membrane through PECVD (plasma enhanced chemical vapor deposition)
CN107083538A
Reaction cavity and processing method thereof
CN113823546A
Method for reducing metal pollution in semiconductor equipment process chamber
CN113846312A
Treatment method of HDPCVD process equipment
CN114242553A
Cited By
Method for forming protective film, protective film, and semiconductor process apparatus
WO2026016919A1