Preparation method of hierarchical mesoporous nickel monatomic catalyst and application of hierarchical mesoporous nickel monatomic catalyst in carbon dioxide electroreduction
By adding weak ligands to the MOF precursor, a fractionated mesoporous carbon support Ni-N-C single-atom catalyst was prepared, which solved the problem of insufficient mass transfer performance in electrocatalytic reduction of carbon dioxide technology, and achieved efficient electroreduction of carbon dioxide to carbon monoxide. The efficiency has been significantly improved.
Patent Information
- Application Number
- CN202411134261.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
AI Technical Summary
Electrocatalytic reduction of carbon dioxide technology faces problems such as chemical inertness, high overpotential, low product selectivity and slow reaction kinetics, especially direct factors affecting performance of catalysts.
The preparation method of the MOF-derived graded mesoporous carbon support Ni-N-C single-atom catalyst is adopted. By adding weak ligands to the MOF precursor, the pyrolysis behavior is improved, and carbon support with different pore structures is constructed to improve the activity and selectivity of the catalyst.
The activity and selectivity of the catalyst are improved, the mass transfer process in the reaction is enhanced, and the efficient electrical reduction of carbon dioxide to carbon monoxide at lower voltages is achieved, and the Faraday efficiency reaches more than 80%.
Smart Images

Figure CN118910651A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrocatalytic reduction of carbon dioxide, and in particular to a preparation method of a graded mesoporous nickel single-atom catalyst and application thereof in electrocatalytic reduction of carbon dioxide. Background Art
[0002] With the rapid development of global population, economy and industry, the environment on which human beings depend for survival has been increasingly polluted. In recent years, the increase in carbon dioxide content in the air has triggered a series of ecological problems such as greenhouse effect, glacier melting and ocean acidification. There are many ways for carbon dioxide to be discharged into the air. One common way is to produce carbon dioxide by burning traditional fossil energy, which not only accelerates the consumption of non-renewable energy on the earth but also interrupts the carbon cycle. Therefore, the development of renewable energy and the reduction of greenhouse gas content in the atmosphere have become urgent needs for human sustainable development. Among them, electro-reduction of carbon dioxide has great application prospects due to its simple operation, wide source of electricity, mild reaction conditions and controllable catalytic process. However, electro-catalytic reduction of carbon dioxide technology still faces many problems. The chemical inertness of carbon dioxide molecules themselves makes them difficult to be activated. In addition, electro-catalytic reduction of carbon dioxide involves a process involving multiple electrons and proton transfer, the required overpotential is high, the selectivity of the product is also low, and there is competition from hydrogen evolution side reactions. Therefore, it is a challenge to find highly active electrocatalysts.
[0003] Non-precious metal single-atom catalysts have been widely used in the study of carbon dioxide electroreduction in recent years due to their advantages such as maximized metal atom utilization, unique quantum size effect, low metal loading, and low cost. However, they still face certain challenges, including the high chemical stability and inertness of CO2 molecules, the complex carbon dioxide electroreduction process, and slow reaction kinetics. So far, researchers have improved their electrocatalytic performance through strategies such as regulating various metal sites and optimizing the coordination structure and environment of active sites. However, the mass transfer performance of the catalyst is a direct factor affecting the performance of the electrocatalyst, and porosity engineering is an effective strategy to construct favorable transfer and enhance the mass transfer capacity of the catalyst. Summary of the invention
[0004] The present invention aims to provide an efficient method for preparing MOF-derived graded mesoporous carbon carrier Ni-NC single-atom catalyst materials, adding weak ligands to the MOF precursor to improve the pyrolysis behavior of ZIF-8, and finally constructing carbon carriers with different pore structures and catalysts with different structures, thereby improving the mass activity of the single-atom catalyst, accelerating the mass transfer process in the reaction, and improving the activity and selectivity of the catalyst.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a hierarchical mesoporous Ni single atom catalyst comprises the following steps:
[0007] S1. Preparation of MOF precursor: Zn(NO3)2·6H2O, 2-methylimidazole and weak ligand were ultrasonically dissolved in methanol and recorded as A, B and C respectively. Then, after stirring at room temperature until completely dissolved, B and C were poured into A solution and stirred at room temperature for 24 hours. The white emulsion obtained by the reaction was washed with methanol for 3 times and dried in a vacuum oven at 60°C to finally obtain a white MOF precursor powder;
[0008] S2. Preparation of nitrogen-doped carbon carrier: After the MOF precursor powder obtained in step S1 is fully ground, it is placed in a tube furnace and heated to 1000°C at 5°C / min under argon atmosphere and maintained for 3 hours, and then cooled to room temperature to obtain a black powder. The black powder is placed in 1M HCl, heated to 80°C in an oil bath and stirred for 12 hours to remove unstable impurities and metals, and then washed with deionized water to neutrality, and the black powder is placed in a 60°C vacuum oven and dried overnight to obtain a graded mesoporous nitrogen-doped carbon material;
[0009] S3. Preparation of hierarchical mesoporous Ni single-atom catalyst: add the isopropanol solution of Ni(NO3)2·6H2O dropwise into the isopropanol solution of nitrogen-doped carbon powder obtained in step S2, heat in an oil bath to 80°C and stir for 6 hours, centrifuge and vacuum dry at 60°C for 12 hours, place in a tubular furnace under argon atmosphere protection at a heating rate of 5°C / min and maintain for 3 hours, anneal at high temperature and cool to room temperature to finally obtain a hierarchical porous Ni single-atom catalyst.
[0010] According to a further technical solution, in step S1, the weak ligand is polyvinyl pyrrolidone (PVP).
[0011] According to a further technical solution, in step S1, the mass ratio of Zn(NO3)2·6H2O to 2-methylimidazole is 1:2.
[0012] According to a further technical solution, in step S1, the mass ratio of the weak ligand to 2-methylimidazole is 0 to 1.9, and the mass ratio of the weak ligand to Zn(NO3)2·6H2O is 0 to 4.0.
[0013] According to a further technical solution, in step S3, the nitrogen-doped carbon powder is 50 mg and the solvent is 25 mL.
[0014] According to a further technical solution, in step S3, the annealing temperature is 700-900°C.
[0015] The application of a hierarchical mesoporous Ni single-atom catalyst prepared by the above-mentioned preparation method in the electroreduction of carbon dioxide to produce carbon monoxide.
[0016] According to a further technical solution, the voltage applied during the electroreduction of carbon dioxide to carbon monoxide is -0.5 to -0.9 V vs. RHE.
[0017] The principle and beneficial effects of this technical solution:
[0018] The present invention adopts the impregnation-pyrolysis method to prepare the Ni-based single-atom catalyst, and uses 3D-MOFs as the precursor. After carbonization, it not only retains the three-dimensional structure of the precursor, but also retains the advantages of large specific surface area and high porosity. 2+ The MOF-8 is assembled as nodes) with rich nitrogen content, high crystallinity and high porosity and simple synthesis method. In the process of preparing ZIF-8, the weak ligand PVP is introduced to form Zn coordination competition with 2-methylimidazole. The in-situ constrained pyrolysis strategy is used to change the pyrolysis behavior of MOF, thereby increasing the content of mesopores in the carbon carrier. The pore size distribution of the Ni single-atom catalyst carbon carrier is regulated by rationally designing the modification process and optimizing the experiment to improve the activity of the catalyst. The process is simple and has good repeatability. By changing the pore size distribution of the single-atom catalyst, the mass transfer process in the catalytic reaction process is improved, thereby improving the activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a flow chart of a method for preparing a hierarchical mesoporous nickel single atom catalyst;
[0020] Figure 2 XRD patterns of ZIF-8 and Ni-based single atom catalyst (Ni-NC);
[0021] Figure 3 TEM of Ni-based single atom catalyst (Ni-NC);
[0022] Figure 4 is the pore size distribution diagram of Ni-based single atom catalyst (Ni-NC);
[0023] Figure 5 This is the Faraday efficiency diagram of the nickel single atom catalyst in Ni-NC at -0.5 to -0.9 V vs. RHE;
[0024] Figure 6 This is the Faraday efficiency diagram of the nickel single atom catalyst in Ni-NC-700 at -0.5 to -0.9 V vs. RHE;
[0025] Figure 7 This is the Faraday efficiency diagram of the nickel single atom catalyst in Ni-NC-900 at -0.5 to -0.9 V vs. RHE;
[0026] Figure 8(a) is the X-ray diffraction analysis spectrum of PVP-8@ZIF-8 precursor and ZIF-8; (b) is the X-ray diffraction analysis spectrum of Ni-NC(P)-8 catalyst;
[0027] Fig. 9 (a) is a transmission electron microscopy (TEM) analysis of Ni-NC(P)-8 catalyst; (b) is a high-resolution transmission electron microscopy (HRTEM) analysis of Ni-NC(P)-8 catalyst;
[0028] (c) High angle annular dark field scanning transmission electron microscopy (HAADF-STEM) analysis of Ni-NC(P)-8 catalyst;
[0029] Fig.10 The pore size distribution diagram of Ni-based single atom catalyst (Ni-NC(P)-8);
[0030] Fig.11 The Faradaic efficiency diagram of Ni-NC(P)-8 catalyst at -0.5 to -0.9 V vs. RHE;
[0031] Fig.12 TOF graphs of Ni-NC catalyst and Ni-NC(P)-8 catalyst.
[0032] Fig.13 The current density diagram of Ni-NC(P)-4 catalyst at -0.5~-0.9V vs.RHE;
[0033] Fig.14 The current density diagram of Ni-NC(P)-12 catalyst at -0.5~-0.9V vs.RHE;
[0034] Fig.15 Schematic diagram of N2 adsorption / desorption analysis of Ni-NC and Ni-NC(P)-8 materials by BET method. DETAILED DESCRIPTION
[0035] The present invention is described in detail below in conjunction with the accompanying drawings and examples, but the present invention is not limited to the following examples, and the preferred embodiments herein are only used to illustrate and explain the present invention. The assay methods not described in detail in the present invention are all routine techniques in the art. It should be understood by those skilled in the art that without certain specific details, the present invention can also be implemented.
[0036] Example 1
[0037] like Figure 1 As shown, a method for preparing a hierarchical mesoporous nickel single-atom catalyst comprises the following steps:
[0038] S1. Preparation of ZIF-8 precursor: dissolve 3.0 g of Zn(NO3)2·6H2O in 40 mL of methanol by ultrasonication to obtain liquid A for use, dissolve 6.0 g of 2-methylimidazole in 80 mL of methanol by ultrasonication to obtain liquid B for use, add liquid B in step A to liquid under vigorous stirring at room temperature and continue stirring for 24 h; centrifuge the white emulsion obtained by the reaction, wash it three times with methanol, and then vacuum dry it at 60 °C for 12 h to obtain white ZIF-8 powder.
[0039] S2. Preparation of nitrogen-doped carbon materials: Grind the ZIF-8 powder obtained in step S1 and place it in a crucible, place it in the middle of a tube furnace, heat it to 1000°C at a rate of 5°C / min in an argon atmosphere, and maintain it at this temperature for 3 hours. After cooling to room temperature, the obtained black powder is acid-washed and stirred in a 1M HCl oil bath at 80°C for 12 hours. After washing with deionized water until neutral, it is vacuum-dried at 60°C to obtain a nitrogen-doped carbon material, recorded as NC.
[0040] S3, preparation of Ni-based single-atom catalyst: 50 mg of NC synthesized in S2 was weighed and dissolved in 25 mL of isopropanol solvent, and 0.025 mmol of Ni(NO3)2·6H2O isopropanol solution was added dropwise under vigorous stirring in an 80°C oil bath, and after centrifugation, it was placed in a vacuum oven at 60°C and dried overnight. The above powder was placed in a tube furnace and heated to 800°C at a rate of 5°C / min under the protection of argon atmosphere, and annealed at this temperature for 3 hours to finally obtain a Ni single-atom catalyst, which was recorded as Ni-NC.
[0041] The prepared ZIF-8 precursor and simulated ZIF-8 were subjected to powder X-ray diffraction analysis to obtain the following spectra: Figure 2 As shown in a. By comparison, it can be seen that the prepared ZIF-8 has the same crystal structure as the simulated one, indicating that the ZIF-8 crystal was successfully prepared.
[0042] The prepared Ni-NC catalyst was subjected to X-ray diffraction analysis, and the spectrum was obtained as follows Figure 2 As shown in (b), no characteristic peaks of the transition metal phase were observed, only the peaks of graphite carbon, which ruled out the existence of metal and metal oxide crystal particles, indicating that the Ni species is likely to exist in a monodisperse state.
[0043] The prepared Ni-NC catalyst was subjected to transmission electron microscopy (TEM) analysis, and the spectrum was obtained as follows Figure 3 As shown in Figure 2, the Ni-NC morphology is a typical rhombic dodecahedron.
[0044] The prepared Ni-NC catalyst was subjected to N2 adsorption / desorption analysis to analyze its pore size distribution, and the spectrum was obtained as follows: Figure 4A large part of the pore volume of the Ni-NC catalyst comes from the micropore region (≤2 nm), as shown by the obvious peak at 1.74 nm.
[0045] Example 2
[0046] In this example, a ZIF-8 precursor and a nitrogen-doped carbon material were prepared in the same manner as in Example 1, except that the annealing temperature in S3 was changed to 700° C., and finally a Ni single atom catalyst was obtained, which was recorded as Ni-NC-700.
[0047] Example 3
[0048] In this example, a ZIF-8 precursor and a nitrogen-doped carbon material were prepared in the same manner as in Example 1, except that the annealing temperature in S3 was changed to 900° C., and finally a Ni single atom catalyst was obtained, which was recorded as Ni-NC-900.
[0049] The catalytic performance of Ni-NC, Ni-NC-700 and Ni-NC-900 catalysts prepared by different annealing temperatures in Example 1, Example 2 and Example 3 in carbon dioxide electroreduction was tested.
[0050] Fabrication of working electrode
[0051] 5 mg of catalyst and 20 μL of 5% Nafion solution were added to 730 μL of ethanol solution and 230 μL of deionized water, and the ink was well dispersed by sonication for 60 min. An equal portion of catalyst ink (100 μL) was evenly dropped on the carbon paper hydrophobic gas diffusion layer (1 cm 2 ) and stored at room temperature overnight to allow the solvent to evaporate. The catalyst loading was 0.5 mg cm -2
[0052] The three-electrode system was used to test the carbon dioxide electroreduction performance, with carbon paper loaded with Ni-NC, Ni-NC-700 and Ni-NC-900 as the working electrode, saturated silver / silver chloride electrode as the reference electrode, platinum electrode as the counter electrode, 0.5M potassium bicarbonate solution as the electrolyte, and H-type cell as the electrolytic cell. A constant potential test was performed, and carbon dioxide gas was introduced to saturate the solution before the test, and the flow rate was maintained at 20mL min -1 The time is 30 minutes. The potential range of the test process is -0.5 to -0.9 V vs. RHE. The gas phase products produced by the reaction are detected by gas chromatography, and the product selectivity is calculated based on this.
[0053] The performance analysis was performed by controlled potential electrolysis, and the gas phase products were detected by gas chromatograph (GC, Shimadzu GC2014), equipped with a thermal conductivity detector (TCD) for H2 quantification and a flame ionization detector (FID) for CO quantification. The Faraday efficiency of CO and H2 was calculated according to the formula.
[0054]
[0055] Where: α: the number of electrons transferred during the reaction, F: Faraday constant (96485℃·mol -1 ), n: amount of substance of the product (mol), I total : total current, t: reaction time.
[0056] Product selectivity distribution Figure 5 (Ni-NC), Figure 6 (Ni-NC-700) and Figure 7 The MOF-derived porous carbon-supported nickel single-atom catalyst has a CO Faradaic efficiency of more than 80% in the potential range of -0.5 to -0.9 V vs. RHE, and the CO Faradaic efficiency reaches the maximum at -0.7 V vs. RHE.
[0057] contrast Figure 5 , Figure 6 and Figure 7 It can be seen that the material has the highest Faraday efficiency of carbon monoxide at an annealing temperature of 800°C, indicating that both low and high temperatures are not conducive to the electroreduction of carbon dioxide to carbon monoxide.
[0058] Example 4
[0059] like Figure 1 As shown, a method for preparing a hierarchical mesoporous nickel single-atom catalyst comprises the following steps:
[0060] S1. Preparation of PVP-8@ZIF-8 precursor: 3.0 g of Zn(NO3)2·6H2O was dissolved in 40 mL of methanol by ultrasonication to obtain liquid A for use, 6.0 g of 2-methylimidazole was dissolved in 80 mL of methanol by ultrasonication to obtain liquid B, and 8.0 g of polyvinylpyrrolidone (PVP) was dissolved in 100 mL of methanol to obtain liquid C. After stirring at room temperature for 24 h, liquid B and liquid C in the step were added to liquid A together with vigorous stirring at room temperature and continued to stir for 24 h; the white emulsion obtained by the reaction was centrifuged, washed three times with methanol, and then vacuum dried at 60°C for 12 h to obtain a white powder of PVP-8@ZIF-8 composite material.
[0061] S2. Preparation of nitrogen-doped carbon materials: The PVP-8@ZIF-8 powder obtained in step S1 was ground and placed in a crucible, which was placed in the middle of a tube furnace. The temperature was raised to 1000°C at a rate of 5°C / min in an argon atmosphere and maintained at this temperature for 3 hours. After cooling to room temperature, the obtained black powder was acid-washed and stirred in a 1M HCl oil bath at 80°C for 12 hours. After washing with deionized water until neutral, it was vacuum-dried at 60°C to obtain a nitrogen-doped carbon material, recorded as NC(P)-8.
[0062] S3, preparation of Ni-based single-atom catalyst: Weigh 50 mg of NC(P)-8 synthesized in S2 above and dissolve it in 25 mL of isopropanol solvent, add 0.025 mmol of Ni(NO3)2·6H2O isopropanol solution dropwise under vigorous stirring in an 80°C oil bath, centrifuge and place in a vacuum oven at 60°C to dry overnight. Place the above powder in a tube furnace and heat it to 800°C at a rate of 5°C / min under the protection of argon atmosphere, and keep it at this temperature for 3 hours to finally obtain a Ni single-atom catalyst, recorded as Ni-NC(P)-8.
[0063] The prepared PVP-8@ZIF-8 precursor and simulated ZIF-8 were subjected to powder X-ray diffraction analysis, and the spectra were as follows: Figure 8 As shown in a. By comparison, PVP-8@ZIF-8 and simulated ZIF-8 have the same X-ray diffraction peak spectrum, proving that fully formed ZIF-8 crystals exist in PVP-8@ZIF-8.
[0064] The prepared Ni-NC(P)-8 catalyst was subjected to X-ray diffraction analysis to obtain a spectrum as shown below: Figure 8 As shown in (b), no characteristic peaks of the transition metal phase were observed, only the peaks of graphite carbon, which ruled out the existence of metal and metal oxide crystals, indicating that the Ni species is likely to exist in a monodisperse state.
[0065] The prepared Ni-NC(P)-8 catalyst was subjected to transmission electron microscopy (TEM) analysis, and the spectrum was obtained as follows Fig. 9 The morphology of Ni-NC(P)-8 is a typical rhombic dodecahedron with rougher edges, indicating the presence of a porous structure. High-resolution transmission electron microscopy (HRTEM) analysis is shown in Figure 1. Fig. 9 As shown in (b), almost no metal nanoparticles or clusters can be observed, indicating that the transition metal single atoms are well dispersed in the single atom catalyst.
[0066] The prepared Ni-NC(P)-8 catalyst was analyzed by high angle annular dark field scanning transmission electron microscopy (HAADF-STEM), and the spectrum was obtained as follows Fig. 9c. Bright spots are observed against the gray-black background of the carbon support, indicating the presence of single Ni atoms without aggregation, and the atomic Ni sites are anchored on the entire carbon structure of Ni-NC(P)-8.
[0067] The prepared Ni-NC(P)-8 catalyst was subjected to N2 adsorption / desorption analysis to analyze its pore size distribution. The spectrum was as follows: Fig.10 The Ni-NC(P)-8 catalyst has an obvious graded pore size distribution, with a prominent peak at 1.75 nm and a broad peak at 3.1 nm, corresponding to micropores and mesopores, respectively, indicating that the introduction of PVP into the precursor changes the pore structure of the catalyst after pyrolysis.
[0068] The catalytic performance of the Ni-NC(P)-8 catalyst prepared in Example 4 was tested in the electroreduction of carbon dioxide.
[0069] The three-electrode system was used to test the carbon dioxide electroreduction performance, with carbon paper loaded with Ni-NC(P)-8 catalyst as the working electrode, saturated silver / silver chloride electrode as the reference electrode, platinum electrode as the counter electrode, 0.5M potassium bicarbonate solution as the electrolyte, and H-type cell as the electrolytic cell. A constant potential test was performed, and carbon dioxide gas was introduced to saturate the solution before the test, and the flow rate was maintained at 20mL·min -1 The time is 30 minutes. The potential range of the test process is -0.5 to -0.9 V vs. RHE. The gas phase products produced by the reaction are detected by gas chromatography, and the product selectivity is calculated from it. The product selectivity distribution is shown in Fig.11 As shown in Figure 2, the Faradaic efficiency of CO of MOF-derived hierarchical porous carbon-supported nickel single-atom catalyst is above 90% in the potential range of -0.5 to -0.9 V vs. RHE, and the Faradaic efficiency of CO reaches the maximum at -0.7 V vs. RHE.
[0070] And contrast Figure 8 It can be seen that in the potential range of -0.5 to -0.9 V vs. RHE, the performance of Ni-NC(P)-8 is better than that of Ni-NC, with a high carbon monoxide Faradaic efficiency (FE CO ) and low hydrogen Faraday efficiency (FE H2 ), their FE CO The differences are very small and are mainly due to their identical Ni-N active sites. To reveal the intrinsic activity of a single Ni site under different carbon forms, the turnover frequency (TOF) of CO production was further calculated.
[0071] According to the Nernst equation (E RHE=E(Ag / AgCl)+0.0591×pH+0.197V,25℃) to calculate all potentials relative to the reversible hydrogen electrode (RHE). The TOF of CO in Ni-NC(P)-8 catalyst is calculated by the following formula
[0072]
[0073] Among them I CO is the partial current for CO production, A; n is the number of electrons transferred; F is the Faraday constant 96485 C·mol -1 , m catalyst is the loading mass of the catalyst on the working electrode, g; W is the weight content of the central metal in the catalyst (wt%); M is the atomic weight of the central metal, g·mol -1 .
[0074] like Fig.12 As shown in Figure 2, Ni-NC(P)-8 has a higher TOF than Ni-NC at all potentials. Specifically, at -0.9 V, its TOF is 31644 h. -1 The FE of Ni-NC(P)-8 catalyst with more mesopores is higher than that of Ni-NC. CO and TOF. This indicates that the CO2RR performance can be improved by increasing the number of mesopores in the catalyst containing a hierarchical porous matrix.
[0075] Example 5
[0076] In this example, nitrogen-doped carbon and Ni-based single-atom catalyst materials were prepared in the same manner as in Example 4, except that the amount of PVP added in the preparation of the S1 composite material was changed to 4.0 g, the obtained composite material was denoted as PVP-4@ZIF-8, the C liquid solvent was 50 mL, and finally a Ni single-atom catalyst was obtained, denoted as Ni-NC(P)-4.
[0077] The catalytic performance of the Ni-NC(P)-4 catalyst prepared in Example 5 was tested in the electroreduction of carbon dioxide.
[0078] The three-electrode system was used to test the carbon dioxide electroreduction performance, with carbon paper loaded with Ni-NC(P)-4 catalyst as the working electrode, saturated silver / silver chloride electrode as the reference electrode, platinum electrode as the counter electrode, 0.5M potassium bicarbonate solution as the electrolyte, and H-type cell as the electrolytic cell. A constant potential test was performed, and carbon dioxide gas was introduced to saturate the solution before the test, and the flow rate was maintained at 20mL min -1The time is 30 minutes. The potential range of the test process is -0.5 to -0.9 V vs. RHE. The gas phase products produced by the reaction are detected by gas chromatography, and the product selectivity is calculated based on this. Fig.13 This is the linear sweep voltammetry curve of Ni-NC(P)-4 catalyst in 0.5M KHCO3 electrolyte saturated with carbon dioxide and argon. Fig.13 The two curves show that the Ni-NC(P)-4 catalyst has good electrochemical CO2 reduction activity.
[0079] Example 6
[0080] In this example, nitrogen-doped carbon and Ni-based single-atom catalyst materials were prepared in the same manner as in Example 4, except that the amount of PVP added in the preparation of the S1 composite material was changed to 12.0 g, the obtained composite material was denoted as PVP-4@ZIF-12, the C liquid solvent was 150 mL, and finally a Ni single-atom catalyst was obtained, denoted as Ni-NC(P)-12.
[0081] The carbon dioxide electroreduction performance test was conducted using a three-electrode system, with the carbon paper loaded with the nickel single atom catalyst obtained in Example 6 of the present invention as the working electrode, the saturated silver / silver chloride electrode as the reference electrode, the platinum electrode as the counter electrode, a 0.5M potassium bicarbonate solution as the electrolyte, and an H-type cell as the electrolytic cell. A constant potential test was conducted, and carbon dioxide gas was introduced to saturate the solution before the test, and the flow rate was maintained at 20 mL min -1 The time is 30 minutes. The potential range of the test process is -0.5 to -0.9 V vs. RHE. The gas phase products produced by the reaction are detected by gas chromatography, and the product selectivity is calculated based on this. Fig.14 This is the linear sweep voltammetry curve of Ni-NC(P)-12 catalyst in 0.5M KHCO3 electrolyte saturated with carbon dioxide and argon. Fig.14 The two curves show that the Ni-NC(P)-12 catalyst has good electrochemical CO2 reduction activity.
[0082] Table 1 Analysis of N2 adsorption / desorption specific surface area of Ni-NC and Ni-NC(P)-8 materials by BET method
[0083]
[0084] The N2 physical adsorption and desorption test can obtain the material specific surface area (SBET), pore size distribution and pore volume parameters determined by the Brunauer-Emmett-Teller method. The physical adsorption and desorption data are obtained by the Micromeritics ASAP2460 specific surface and porosity analyzer N2 adsorption and desorption test at 77K. The degassing temperature and time of the sample are 180℃ and 8h respectively. Fig.15 The results are shown in Table 1. The results show that the adsorption isotherms of Ni-NC and Ni-NC(P)-8 exhibit typical type IV adsorption isotherms. Both catalysts are mainly composed of micropores. Compared with the two, Ni-NC has a higher specific surface area of 938.5918 m 2 / g, while the surface area of Ni-NC(P)-8 is 930.9932m 2 Although the many micropores of Ni-NCs may render the loaded active sites inaccessible.
[0085] Table 2 Inductively coupled plasma optical emission spectra (ICP-OES) of Ni-NC and Ni-NC(P)-8
[0086]
[0087] Inductively coupled plasma-optical emission spectroscopy can be used to quantitatively analyze the element content in the sample. The instrument model used is Agilent 5110 (OES). In a typical ICP procedure, 5 mg of sample is added to a mixed solution of 3 mL of concentrated nitric acid and 3 mL of perchloric acid, mixed evenly, heated to 180 ° C until the solution is clear and transparent, cooled and diluted to 50 mL with deionized water and sampled for analysis. As shown in Table 2, the results show that the Ni content of the two catalysts is similar, Ni-NC is 0.26%, and Ni-NC(P)-8 is 0.14%.
[0088] Table 3 Comparison results of synthesized nickel SACs with different nitrogen contents
[0089]
[0090] X-ray photoelectron spectroscopy can not only provide the elemental composition of several to dozens of atomic layers on the surface of solid materials, but also be used to determine the chemical state of elements and perform semi-quantitative analysis. The instrument model used for the test is AXIS SUPRA, and the binding energy of all elements was corrected using the C1s binding energy of other carbons (284.8eV) before analyzing the data.
[0091] The N1s fine spectra of each catalyst were analyzed, and the percentage of each N configuration is shown in Table 3. When the coordination temperature increases, the Ni-N content remains unchanged. However, changes in the pyridinic nitrogen content are observed, and the pyridinic nitrogen content is the highest at a coordination temperature of 800°C. Pyridinic nitrogen (Pyridinic-N) can effectively convert CO2 into CO because they can combine CO2 and protons.
[0092] Table 4 R of all catalysts s and R ct
[0093]
[0094]
[0095] Resistance is the magnitude of the resistance to electric current in a circuit, and is numerically equal to voltage / current. An ideal resistor satisfies the following relationship and follows Ohm's law. The resistance value is independent of frequency. However, in reality, the properties of many circuit elements are more complex, so a more commonly used circuit element, impedance, has to be used. Unlike current, impedance is affected by frequency. Impedance testing is generally measured using a small-amplitude AC signal excitation, and its magnitude is also expressed as the magnitude of the circuit's resistance to current. In electrochemical systems, EIS is not only used to characterize electrochemical processes, such as electrode kinetics, interfacial double layers, etc., but also as an electrochemical device optimization tool for material selection, electrochemical corrosion protection, etc. Electrochemical impedance spectroscopy (EIS) analysis was performed at a potential of -0.7V vs. RHE, with an amplitude of 5mV and a test frequency range of 0.1Hz to 100kHz. The data obtained from the test was fitted and analyzed. Table 4 shows the fitting results of electrochemical impedance, R s is the solution resistance, R ct is the catalyst interface resistance, R ct The lower the value, the faster the charge transfer within the surface system, which corresponds to the CO2 reduction performance of the catalyst.
[0096] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for preparing a hierarchical mesoporous Ni single atom catalyst, characterized in that the steps are as follows: S1. Preparation of MOF precursor: Zn(NO3)2·6H2O, 2-methylimidazole and weak ligand were ultrasonically dissolved in methanol and recorded as A, B and C respectively. Then, after stirring at room temperature until completely dissolved, B and C were poured into A solution and stirred at room temperature for 24 hours. The white emulsion obtained by the reaction was washed with methanol for 3 times and dried in a vacuum oven at 60°C to finally obtain a white MOF precursor powder; S2. Preparation of nitrogen-doped carbon carrier: After the MOF precursor powder obtained in step S1 is fully ground, it is placed in a tube furnace and heated to 1000°C at 5°C / min under argon atmosphere and maintained for 3 hours, and then cooled to room temperature to obtain a black powder. The black powder is placed in 1M HCl, heated to 80°C in an oil bath and stirred for 12 hours to remove unstable impurities and metals, and then washed with deionized water to neutrality, and the black powder is placed in a 60°C vacuum oven and dried overnight to obtain a hierarchical porous nitrogen-doped carbon material; S3. Preparation of hierarchical mesoporous Ni single-atom catalyst: add the isopropanol solution of Ni(NO3)2·6H2O dropwise into the isopropanol solution of nitrogen-doped carbon powder obtained in step S2, heat in an oil bath to 80°C and stir for 6 hours, centrifuge and vacuum dry at 60°C for 12 hours, place in a tubular furnace under argon atmosphere protection at a heating rate of 5°C / min and maintain for 3 hours, anneal at high temperature and cool to room temperature to finally obtain a hierarchical porous Ni single-atom catalyst.
2. The method for preparing a hierarchical mesoporous Ni single-atom catalyst according to claim 1, characterized in that: In the step S1, the weak ligand is polyvinyl pyrrolidone (PVP).
3. The method for preparing a hierarchical mesoporous Ni single-atom catalyst according to claim 1 or 2, characterized in that: In the step S1, the mass ratio of Zn(NO3)2·6H2O to 2-methylimidazole is 1:
2.
4. The method for preparing a hierarchical mesoporous Ni single atom catalyst according to claim 1 or 2, characterized in that: In the step S1, the mass ratio of the weak ligand to 2-methylimidazole is 0 to 1.9, and the mass ratio of the weak ligand to Zn(NO3)2·6H2O is 0 to 4.
0.
5. The method for preparing a hierarchical mesoporous Ni single atom catalyst according to claim 1 or 2, characterized in that: In the step S3, the nitrogen-doped carbon powder is 50 mg and the solvent is 25 mL.
6. The method for preparing a hierarchical mesoporous Ni single atom catalyst according to claim 1 or 2, characterized in that: In the step S3, the annealing temperature is 700-900°C.
7. Use of a hierarchical mesoporous Ni single-atom catalyst prepared by the preparation method according to any one of claims 1 to 6 in the electroreduction of carbon dioxide to generate carbon monoxide.
8. The use according to claim 7, characterized in that: The voltage applied during the electroreduction of carbon dioxide to carbon monoxide is -0.5 to -0.9 V vs. RHE.
Citation Information
Cited By
HOF-derived thin-walled carbon nanotube loaded nickel monatomic catalyst and preparation method and application thereof
CN119776883A
A highly dispersed nickel-based carbon-nitrogen catalyst, preparation method and application thereof
CN120400890B