Molybdenum cation and phosphorus anion co-doped VS2 catalytic material as well as preparation method and application thereof in hydrogen evolution reaction

The vanadium disulfide material co-doped with molybdenum cation and phosphorus anion forms a nanosheet-like flower-like structure on carbon-based materials, solving the problem of poor stability of vanadium disulfide material and achieving efficient electrocatalytic hydrogen evolution reaction. Excellent catalytic activity and stability.

CN118910654AActive Publication Date: 2024-11-08XIANGTAN UNIV

Patent Information

Application Number
CN202410730868.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-11-08
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

The existing vanadium disulfide materials have poor stability in electrocatalytic hydrogen evolution reactions. Although doping can improve catalytic activity, they cannot effectively solve the problem of insufficient cycle stability.

Method used

The vanadium disulfide catalytic material co-doped with molybdenum cation and phosphorus anion is used to form a nanosheet-shaped flower-like structure on the carbon-based material to improve catalytic activity and stability, and dopant through hydrothermal and heat treatment. Achieve efficient electrocatalytic hydrogen evolution reaction.

Benefits of technology

It achieves high HER catalytic activity and excellent stability in electrocatalytic hydrogen evolution reaction, low overpotential and small Taffir slope, and only slightly attenuated polarization after long-term cyclic voltammetry scanning and constant current polarization, which is significant Improves the circulation stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910654A_ABST
    Figure CN118910654A_ABST
Patent Text Reader

Abstract

The invention discloses a molybdenum cation and phosphorus anion co-doped VS2 catalytic material as well as a preparation method and application thereof in hydrogen evolution reaction, and belongs to the technical field of electro-catalytic materials. The catalytic material is formed by uniformly growing microflowers on a carbon-based material; the preparation method comprises the following steps: firstly, carrying out oxidation pretreatment on the surface of a carbon-based material, then growing a molybdenum-doped vanadium disulfide material on the surface of the carbon-based material in situ through a hydrothermal method, and doping phosphorus through a heat treatment method, so as to obtain the molybdenum-doped vanadium disulfide / carbon-based composite material. The molybdenum cation and phosphorus anion co-doped VS2 catalytic material with excellent HER catalytic activity and cycling stability is obtained, and the preparation method is simple in process, low in cost, high in yield, mild in condition, simple in needed equipment, environmentally friendly and beneficial to industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a modified VS2 catalytic material, in particular to a molybdenum cation and a phosphorus anion co-doped VS2 catalytic material, and also to a preparation method thereof and application in an electrocatalytic hydrogen evolution reaction, belonging to the technical field of electrocatalytic materials. Background Art

[0002] Commercial Pt-based HER catalysts are recognized as the most efficient catalysts for hydrogen production by water electrolysis due to their excellent catalytic activity and stability. However, Pt is a precious metal, and its high cost and low earth reserves severely limit the development of the water electrolysis hydrogen production industry. Therefore, the development of catalytic materials of non-precious metal elements has become a hot topic in the field of water electrolysis catalytic materials.

[0003] At present, transition metal sulfides (TMDs) have attracted the interest of researchers due to their large specific surface area and high catalytic activity edge. As a representative of transition metal sulfides, vanadium disulfide (VS2) is regarded as a promising HER catalyst that can replace the precious metal Pt because of its metallic properties, catalytic activity at both edges and in-plane, and low cost. The literature (Chemical Engineering Journal, 2020, 396: 125227) discloses that Mo cation doping can significantly enhance the in-plane hydrogen evolution activity of VS2, and in addition to Mo doping, metal cation doping with low hydrogen adsorption free energy such as Ni and Co has also been shown to enhance the HER activity of VS2, such as literature: (Small 2024, 2311217), (International Journal of Hydrogen Energy, 2022, 47 (19): 10646-10653.), (Journal of Materials Chemistry A, 2022, 10 (16): 9067-9079.) and so on. At present, most vanadium disulfide or transition metal doped vanadium disulfide materials are synthesized by hydrothermal method. However, vanadium disulfide materials synthesized by hydrothermal method generally have the technical problem of poor cycle stability, for example, reference (ACS applied materials & interfaces, 2017, 9 (48): 42139-42148). It is reported in the prior art that doping vanadium disulfide materials with transition metal ions can improve their HER activity, but it cannot solve the technical problem of poor stability. Summary of the invention

[0004] In view of the defects of the prior art, the first object of the present invention is to provide a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions, which has not only good stability but also high HER catalytic activity.

[0005] The second object of the present invention is to provide a method for preparing a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions. The preparation method is simple, low-cost, and has a low synthesis temperature. It does not require large equipment and harsh reaction conditions, and can achieve large-scale production.

[0006] The third object of the present invention is to provide an application of a VS2 catalyst material co-doped with a molybdenum cation and a phosphorus anion, which is used as an electrocatalytic active material in an electrocatalytic hydrogen evolution reaction, showing excellent hydrogen evolution performance and stability, for example, at 50 mA cm -2 The overpotential is as low as -0.2303 V (relative to standard hydrogen electrode) at the current density, and the Tafel slope is as low as 49.5 mV / dec. After 10,000 CV scans, the polarization curve is at 50 mA cm -2 The current density of -2 After 120 hours of constant current polarization at the current density, the overpotential only decayed by 40mV.

[0007] In order to achieve the above technical objectives, the present invention provides a molybdenum cation and phosphorus anion co-doped VS2 catalytic material, which is composed of micron flowers uniformly grown on a carbon-based material; the micron flowers are assembled from molybdenum cation and phosphorus anion co-doped VS2 nanosheets.

[0008] The VS2 catalytic material co-doped with molybdenum cations and phosphorus anions of the present invention has a special flower-like structure, which is formed by self-assembly of nano-sheet molybdenum cations and phosphorus anions co-doped with VS2 to form a micrometer-sized flower-like structure uniformly grown on a carbon-based material. The catalytic material uses the carbon-based material as a carrier, which can achieve high dispersion and stable loading of catalytic active components, increase the specific surface area of ​​the catalytic active components, expose more catalytic active sites, and thus have better catalytic activity, and can improve the stability and conductivity of the catalytic material. The micro-flowers formed by the self-assembly of nanosheet-shaped molybdenum cations and phosphorus anions co-doped VS2 are used as catalytic active components. The micro-flower structure has a large specific surface area, many exposed active sites, and better catalytic activity. The doping of molybdenum cations can reduce the diameter of the micro-flowers, increase its specific surface area, regulate the electronic structure of vanadium disulfide, expand the interlayer spacing of the layered structure of vanadium disulfide micro-flowers, increase the number of its active sites, and significantly improve its electrocatalytic hydrogen evolution activity and cycle stability. In particular, phosphorus anions are also doped at the same time. Since molybdenum cation doping enhances the adsorption of hydrogen on the S site of the substrate plane, it also inevitably enhances the adsorption of hydrogen on the S site of the V edge, which leads to over-binding of H*, which is not conducive to the HER of the V edge site after molybdenum cation doping. The introduction of phosphorus anions into molybdenum cation-doped VS2 can compensate for the excessive adsorption of H* on the in-plane sites and edge sites of molybdenum cation doping, thereby moderately weakening their adsorption activity for H*. At the same time, it is unexpectedly found that phosphorus doping can significantly improve the stability of molybdenum-doped vanadium disulfide materials.

[0009] As a preferred solution, the micro-flowers grow into a layered structure. The growth of micro-flowers into a layered structure can increase the number of catalytic active sites.

[0010] As a preferred solution, the carbon-based material is carbon cloth. The preferred carbon-based material is carbon cloth, which is flexible and has a porous structure, and is more suitable as a carrier material for the VS2 catalytic active component.

[0011] As a preferred solution, in the co-doped VS2 of molybdenum cations and phosphorus anions, the doping amount of molybdenum cations is measured by the atomic ratio of Mo to V (0.05-0.15): (0.95-0.85), and the doping amount of phosphorus anions is measured by the atomic ratio of P to S (0.01-0.15): (0.99-0.85). The hydrogen evolution performance of molybdenum-doped vanadium disulfide first increases and then decreases with the doping amount of molybdenum, and the hydrogen evolution performance is close to the best when the molybdenum doping amount is 10%. On the basis of molybdenum doping, phosphorus anions are further doped. The hydrogen evolution performance of VS2 co-doped with molybdenum cations and phosphorus anions is improved with the increase of phosphorus doping amount. When the phosphorus anion content increases to a certain extent, the hydrogen evolution performance shows a downward trend.

[0012] The molybdenum-doped vanadium disulfide micro-flower material of the present invention contains four elements: Mo, V, S, and P, and its physical phase is a single vanadium disulfide physical phase. Molybdenum cations are doped in the VS2 lattice to replace vanadium cations, and phosphorus anions are doped in the VS2 lattice to replace sulfur anions.

[0013] The present invention also provides a method for preparing a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions, the method comprising the following steps:

[0014] 1) performing oxidation pretreatment on the surface of the carbon-based material to obtain a pretreated carbon-based material;

[0015] 2) adding a molybdenum source, a vanadium source and ammonia water into water, stirring until transparent, and then adding a sulfur source and stirring to obtain a mixed solution; transferring the mixed solution into a reactor containing a pretreated carbon-based material, performing a hydrothermal reaction, and obtaining a molybdenum-doped vanadium disulfide material;

[0016] 3) Using sodium hypophosphite as a phosphorus source, phosphorus-doping the molybdenum-doped vanadium disulfide material is performed through a heat treatment method to obtain the obtained material.

[0017] The preparation method of the VS2 catalytic material co-doped with molybdenum cations and phosphorus anions of the present invention selects a carbon-based material as a carrier, performs surface oxidation pretreatment on the carbon-based material, which is conducive to the in-situ growth and highly dispersed loading of the VS2 catalytic active components on its surface, and then in-situ deposits a molybdenum-doped vanadium disulfide material on the surface of the carbon-based material by a hydrothermal method. The hydrothermal method can control the morphology of the VS2 crystal and the doping effect of the molybdenum cations, so that it forms a flower-like structure assembled by nanosheets, and the molybdenum cations can be uniformly doped in the VS2 lattice. Finally, the molybdenum-doped vanadium disulfide material is doped with phosphorus by a heat treatment method, and the heat treatment method can achieve uniform and controllable doping of phosphorus.

[0018] As a preferred solution, the oxidation pretreatment process is: soaking the carbon-based material in a mixed acid of nitric acid and sulfuric acid. After the pre-oxidation treatment, oxygen-containing polar groups can be generated on the surface of the carbon-based material, thereby increasing the wettability of the solution to it, which is beneficial to in-situ deposition. At the same time, the polar groups can coordinate and bind vanadium ions in the solution, which is beneficial to the in-situ growth of VS2 and prevents agglomeration. The mixed acid of nitric acid and sulfuric acid is a mixed acid composed of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 2.5 to 3.5:1. The soaking time is preferably more than 12 hours.

[0019] As a preferred solution, the molybdenum source includes at least one of ammonium molybdate, sodium molybdate and potassium molybdate.

[0020] As a preferred solution, the vanadium source includes ammonium metavanadate and / or sodium vanadate.

[0021] As a preferred embodiment, the sulfur source includes thiourea and / or thioacetamide.

[0022] The molybdenum source, vanadium source, sulfur source and phosphorus source involved in the present invention are all conventional commercial reagents in the prior art.

[0023] As a preferred solution, the molybdenum source, vanadium source and sulfur source are measured according to the atomic ratio of molybdenum, vanadium and sulfur of (0.05-0.15):(0.95-0.85):(5-10).

[0024] As a preferred solution, the mass ratio of the phosphorus source to the molybdenum-doped vanadium disulfide material is 1.2 to 1.7:1

[0025] As a preferred solution, the conditions of the hydrothermal reaction are: temperature of 140-220°C and time of 12-26 hours. The most preferred hydrothermal reaction temperature is 160-180°C; the most preferred hydrothermal reaction time is 23-25 ​​hours.

[0026] As a preferred scheme, the process of phosphorus-doping the molybdenum-doped vanadium disulfide material by heat treatment is as follows: sodium hypophosphite is placed in the upstream heating zone of the tubular furnace, and the molybdenum-doped vanadium disulfide material is placed in the downstream heating zone of the tubular furnace. An inert atmosphere is filled into the tubular furnace, and the temperature of the upstream heating zone is controlled to be 300-350°C, and the temperature of the downstream heating zone is controlled to be 300-500°C. After keeping warm for 2-4 hours, the mixture is cooled to room temperature.

[0027] The preparation method of the VS2 catalytic material co-doped with molybdenum cations and phosphorus anions of the present invention is illustrated below:

[0028] 1) First step: Carbon cloth (CC) treatment: Cut the carbon cloth into rectangular pieces of 1 cm × 1.5 cm in size, soak the carbon cloth in nitric acid-sulfuric acid mixed acid, ultrasonically wash it with deionized water and anhydrous ethanol for more than three times, and then dry it in a vacuum drying oven;

[0029] 2) The second step is to synthesize Mo-doped VS2: add a molybdenum source, a vanadium source and ammonia water into water, stir until transparent, then add a sulfur source, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, and then subject the mixed solution to a one-step hydrothermal reaction. The reaction product is washed and dried to obtain a molybdenum-doped vanadium disulfide precursor material;

[0030] 3) The third step is to perform P doping by heat treatment: sodium hypophosphite is used as the P doping source, and the sodium hypophosphite is placed in a magnetic boat at the center of the upstream heating zone of the tubular furnace, and the above-mentioned molybdenum-doped vanadium disulfide precursor material is placed in the magnetic boat, and placed in the center of the downstream heating zone; in an argon atmosphere, heating is performed, and the temperatures of the upper temperature zone and the lower temperature zone are 300°C and 300-500°C, respectively. After keeping warm for a period of time and cooling to room temperature, a VS2 electrocatalytic electrode material co-doped with molybdenum cations and phosphorus anions is obtained.

[0031] The drying involved in the present invention adopts vacuum freeze drying or vacuum drying at 50-80°C.

[0032] The present invention also provides an application of a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions, which is applied to an electrocatalytic hydrogen evolution reaction.

[0033] The molybdenum cation and phosphorus anion co-doped VS2 catalyst material provided by the present invention is applied to the electrocatalytic hydrogen evolution reaction and exhibits excellent hydrogen evolution performance at 50 mA cm -2 The overpotential is as low as -0.2303 V (relative to standard hydrogen electrode) at the current density, and the Tafel slope is as low as 49.5 mV / dec. After 10,000 CV scans, the polarization curve is at 50 mA cm -2 The current density of -2 After 120 hours of constant current polarization at the current density, the overpotential only decayed by 40mV.

[0034] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0035] 1) The molybdenum cation and phosphorus anion co-doped VS2 catalytic material provided by the present invention is composed of nano-sheet molybdenum cations and phosphorus anions co-doped VS2 self-assembled to form a micrometer-sized flower-like structure uniformly grown on a carbon-based material, which exhibits high electrocatalytic hydrogen evolution activity and stability; at 50 mA cm -2 The overpotential is as low as -0.2303 V (relative to standard hydrogen electrode) at the current density, and the Tafel slope is as low as 49.5 mV / dec. After 10,000 CV scans, the polarization curve is at 50 mA cm -2 The current density of -2 After 120 hours of constant current polarization at the current density, the overpotential only decayed by 40mV.

[0036] 2) The preparation method of the molybdenum cation and phosphorus anion co-doped VS2 catalytic material provided by the present invention is simple, low-cost, and the reaction conditions are easy to control, which can meet the advantages of industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 XRD patterns of the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions in Examples 1 to 3 of the present invention, the Mo-doped VS2 catalyst material in Comparative Example 1, the P-doped VS2 catalyst material in Comparative Example 2, and the undoped vanadium disulfide catalyst material in Comparative Example 3.

[0038] Figure 2This is the SEM spectrum of the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions in Example 1 of the present invention. Figure 3 This is an EDS surface scan analysis of the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions in Example 1 of the present invention.

[0039] Figure 4 Polarization curves (after iR compensation) of the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions in Examples 1 to 3 of the present invention, the Mo-doped VS2 catalyst material in Comparative Example 1, the P-doped VS2 catalyst material in Comparative Example 2, and the undoped vanadium disulfide catalyst material in Comparative Example 3 in 0.5 mol / L sulfuric acid solution.

[0040] Figure 5 Tafel plots of the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions in Examples 1 to 3 of the present invention, the Mo-doped VS2 catalyst material in Comparative Example 1, the P-doped VS2 catalyst material in Comparative Example 2, and the undoped vanadium disulfide catalyst material in Comparative Example 3 in 0.5 mol / L sulfuric acid solution.

[0041] Figure 6 This is the cyclic voltammetry curve of the VS2 hydrogen evolution electrocatalyst co-doped with molybdenum cations and phosphorus anions in Example 1 of the present invention in a 0.5 mol / L sulfuric acid solution.

[0042] Figure 7 This is the cyclic voltammetry curve of the VS2 hydrogen evolution electrocatalyst co-doped with molybdenum cations and phosphorus anions in Example 2 of the present invention in a 0.5 mol / L sulfuric acid solution.

[0043] Figure 8 This is the cyclic voltammetry curve of the VS2 hydrogen evolution electrocatalyst co-doped with molybdenum cations and phosphorus anions in Example 3 of the present invention in 0.5 mol / L sulfuric acid solution.

[0044] Fig. 9 This is the cyclic voltammetry curve of the Mo-doped VS2 hydrogen evolution electrocatalyst in 0.5 mol / L sulfuric acid solution in Comparative Example 1 of the present invention.

[0045] Fig.10 This is the cyclic voltammetry curve of the P-doped VS2 hydrogen evolution electrocatalyst in 0.5 mol / L sulfuric acid solution in Comparative Example 2 of the present invention.

[0046] Fig.11 This is the cyclic voltammetry curve of pure VS2 hydrogen evolution electrocatalyst in 0.5 mol / L sulfuric acid solution in comparative embodiment 3 of the present invention.

[0047] Fig.12The CV curves of the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions in Examples 1 to 3 of the present invention, the Mo-doped VS2 catalyst material in Comparative Example 1, the P-doped VS2 catalyst material in Comparative Example 2 and the undoped vanadium disulfide catalyst material in Comparative Example 3 in 0.5 mol / L sulfuric acid solution are the capacitance current density-scan rate changes at a potential of 0.2 V, and the straight line is the fitting result.

[0048] Fig.13 Polarization curves of the VS2 hydrogen evolution electrocatalyst co-doped with molybdenum cations and phosphorus anions in Example 1 of the present invention before and after CV stability in a 0.5 mol / L sulfuric acid solution.

[0049] Fig.14 This is the voltage-time curve of the constant current polarization of the VS2 hydrogen evolution electrocatalyst co-doped with molybdenum cations and phosphorus anions in Example 1 of the present invention in a 0.5 mol / L sulfuric acid solution.

[0050] Fig.15 This is the SEM morphology of the undoped vanadium disulfide micro-flower material in Comparative Example 3 of the present invention.

[0051] Fig.16 This is the EDS surface scanning analysis of the undoped vanadium disulfide micro-flower material in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0052] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner in conjunction with the accompanying drawings and preferred embodiments of the present invention.

[0053] Embodiment 1:

[0054] 1) First step: Carbon cloth (CC) treatment: Cut the carbon cloth into rectangular pieces of 1 cm × 1.5 cm in size, soak the carbon cloth in a mixed acid of nitric acid and sulfuric acid in a ratio of 3:1 for more than 12 hours, then ultrasonically wash it with deionized water and anhydrous ethanol for more than three times, and then dry it in a vacuum drying oven at 60°C;

[0055] 2) The second step is to synthesize the Mo-doped VS2 precursor, the preparation method of which is to weigh 0.2106g of ammonium metavanadate, 0.0353g of ammonium molybdate and 2ml of ammonia water, add them to water, stir and dissolve into a transparent solution, then weigh 1.5026g of thioacetamide and add it to the above transparent solution, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, pour the liquid into a polytetrafluoroethylene liner and seal it, then put the polytetrafluoroethylene liner into a stainless steel reactor and tighten it, and then place it in an oven at 160°C for 24 hours. After naturally cooling to room temperature, wash the obtained product with anhydrous ethanol and deoxygenated deionized water in turn; then put it in a refrigerator and freeze it for 12 hours, and then place it in a freeze dryer at -50°C for vacuum drying for 30 hours to obtain a molybdenum-doped vanadium disulfide precursor material;

[0056] 3) The third step is to perform P doping by heat treatment, wherein sodium hypophosphite is used as the P doping source, 0.4 g of sodium hypophosphite is placed in a magnetic boat at the center of the upstream heating zone of a tubular furnace, and a whole piece of the molybdenum-doped vanadium disulfide precursor material is placed in the magnetic boat and placed in the center of the downstream heating zone; in an argon atmosphere, the temperature of the upstream heating zone is controlled to be 300°C, and the temperature of the downstream heating zone is controlled to be 400°C, and the temperature is kept for 3 hours. After cooling to room temperature, a VS2 electrocatalytic electrode material co-doped with molybdenum cations and phosphorus anions is obtained.

[0057] X-ray diffractometer (XRD) was used to characterize the structure of the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material obtained above, as shown in FIG. Figure 1 As shown, the results show that the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is a single vanadium disulfide phase without other impurity phases, and its 011 plane is shifted to the left due to P doping; the morphology of the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is characterized by scanning electron microscopy (SEM), as shown Figure 2 As shown in the figure, it can be seen that the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is formed by self-assembly of nano-sheet molybdenum cation and phosphorus anion co-doped VS2 catalyst material to form a micron-sized flower-like structure uniformly grown on a carbon cloth substrate, and the molybdenum cation and phosphorus anion co-doped VS2 catalyst material is subjected to surface scanning analysis by an energy dispersive spectrometer (EDS), as shown in FIG. Figure 3 As shown, the results show that the material contains four elements, Mo, P, V, and S, and they are evenly distributed.

[0058] The electrochemical hydrogen evolution performance of the molybdenum cation and phosphorus anion co-doped VS2 catalyst material was tested using a three-electrode system, with a carbon rod as the counter electrode, a Hg|Hg2SO4 electrode as the reference electrode, a molybdenum cation and phosphorus anion co-doped VS2 catalyst material as the working electrode, and a 0.5 mol / L sulfuric acid solution as the electrolyte. The test instrument was the Shanghai Chenhua CHI660E electrochemical workstation. The linear scan range of the linear scan voltammetry curve was between -1.0 and 0 V (relative to the standard hydrogen electrode), and the scan rate was 3 mV / s. All tests were performed in a constant temperature 25°C water bath environment. The test results are shown in Figure 2. Figure 5 and Figure 6 As shown, after data processing and calculation, at 50mAcm -2 The overpotential is as low as -0.2303V (relative to standard hydrogen electrode) and the Tafel slope is as low as 49.5mV / dec at the current density. The linear scanning range of the linear cyclic voltammetry curve is between 0.15 and 0.25V (relative to standard hydrogen electrode). Figure 6As shown, it can be seen that the CV curves of all materials are rectangular in shape, indicating that no redox reaction occurs. Fig.12 The capacitive current density (Δj = j a -j b , where j a and j b It shows the relationship between the current density in the CV curve at 0.20V (relative to the standard hydrogen electrode) and the scan rate and its linear fitting function. Sample C dl The value is equal to half of the slope of the straight line in the figure, and its C dl The value is 107mF cm -2 . Fig.13 The polarization curves of the sample before and after 5000 CV cycles are shown in Figure 2. Compared with the initial polarization curve, the polarization curve of the sample after 5000 CV cycles is 30 mA cm -2 When , the overpotential only increases by 22mV, indicating that the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions has excellent hydrogen evolution stability. Fig.14 For samples at 10 mA cm -2 From the potential-time curve of the constant current polarization test for 120 h at a current density of , it can be seen that the overpotential of the sample only dropped by 4 mV after a long period of constant current polarization test, indicating that the VS2 catalyst material co-doped with molybdenum cations and phosphorus anions has excellent hydrogen evolution stability.

[0059] Embodiment 2:

[0060] 1) First step: Carbon cloth (CC) treatment: Cut the carbon cloth into rectangular pieces of 1 cm × 1.5 cm in size, soak the carbon cloth in a mixed acid of nitric acid and sulfuric acid in a ratio of 3:1 for more than 12 hours, then ultrasonically wash it with deionized water and anhydrous ethanol for more than three times, and then dry it in a vacuum drying oven at 60°C;

[0061] 2) The second step is to synthesize the Mo-doped VS2 precursor, the preparation method of which is to weigh 0.2106g of ammonium metavanadate, 0.0353g of ammonium molybdate and 2ml of ammonia water, add them to water, stir and dissolve into a transparent solution, then weigh 1.5026g of thioacetamide and add it to the above transparent solution, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, pour the liquid into a polytetrafluoroethylene liner and seal it, then put the polytetrafluoroethylene liner into a stainless steel reactor and tighten it, and then place it in an oven at 160°C for 24 hours. After naturally cooling to room temperature, wash the obtained product with anhydrous ethanol and deoxygenated deionized water in turn; then put it in a refrigerator and freeze it for 12 hours, and then place it in a freeze dryer at -50°C for vacuum drying for 30 hours to obtain a molybdenum-doped vanadium disulfide precursor material;

[0062] 3) The third step is to perform P doping by heat treatment, wherein sodium hypophosphite is used as the P doping source, 0.4 g of sodium hypophosphite is placed in a magnetic boat at the center of the upstream heating zone of a tubular furnace, and a whole piece of the molybdenum-doped vanadium disulfide precursor material is placed in the magnetic boat and placed in the center of the downstream heating zone; in an argon atmosphere, the temperature of the upstream heating zone is controlled to be 300°C, and the temperature of the downstream heating zone is controlled to be 300°C, and the temperature is kept at this temperature for 3 hours. After cooling to room temperature, a VS2 electrocatalytic electrode material co-doped with molybdenum cations and phosphorus anions is obtained.

[0063] X-ray diffractometer (XRD) was used to characterize the structure of the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material obtained above, as shown in FIG. Figure 1 As shown, the results show that the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is a single vanadium disulfide phase without other impurity phases, and its 011 plane shifts to the left due to P doping; SEM is used to characterize the morphology of the above-mentioned molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material. The molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is self-assembled by nano-sheet molybdenum cation and phosphorus anion co-doped VS2 catalyst material to form a micron-sized flower-like structure uniformly grown on a carbon cloth substrate. EDS is used to perform surface scanning analysis on the above-mentioned molybdenum cation and phosphorus anion co-doped VS2 catalyst material. The results show that the material contains four elements, Mo, P, V, and S, and they are uniformly distributed.

[0064] The electrochemical hydrogen evolution performance of the molybdenum cation and phosphorus anion co-doped VS2 catalyst material was tested using a three-electrode system, with a carbon rod as the counter electrode, a Hg|Hg2SO4 electrode as the reference electrode, a molybdenum cation and phosphorus anion co-doped VS2 catalyst material as the working electrode, and a 0.5 mol / L sulfuric acid solution as the electrolyte. The test instrument was the Shanghai Chenhua CHI660E electrochemical workstation. The linear scan range of the linear scan voltammetry curve was between -1.0 and 0 V (relative to the standard hydrogen electrode), and the scan rate was 3 mV / s. All tests were performed in a constant temperature 25°C water bath environment. The test results are shown in Figure 2. Figure 5 and Figure 6 As shown, after data processing and calculation, at 50 mA cm -2 The overpotential is as low as -0.2415V (relative to standard hydrogen electrode) and the Tafel slope is as low as 54.1mV / dec at the current density. The linear scanning range of the linear cyclic voltammetry curve is between 0.15 and 0.25V (relative to standard hydrogen electrode). Figure 7 As shown, it can be seen that the CV curves of all materials are rectangular in shape, indicating that no redox reaction occurs. Fig.12 The capacitive current density (Δj = j a -j b , where j aand j b It shows the relationship between the current density in the CV curve at 0.20V (relative to the standard hydrogen electrode) and the scan rate and its linear fitting function. Sample C dl The value is equal to half of the slope of the straight line in the figure, and its C dl The value is 93.6mF cm -2 .

[0065] Embodiment 3:

[0066] 1) First step: Carbon cloth (CC) treatment: Cut the carbon cloth into rectangular pieces of 1 cm × 1.5 cm in size, soak the carbon cloth in a mixed acid of nitric acid and sulfuric acid in a ratio of 3:1 for more than 12 hours, then ultrasonically wash it with deionized water and anhydrous ethanol for more than three times, and then dry it in a vacuum drying oven at 60°C;

[0067] 2) The second step is to synthesize the Mo-doped VS2 precursor, the preparation method of which is to weigh 0.2106g of ammonium metavanadate, 0.0353g of ammonium molybdate and 2ml of ammonia water, add them to water, stir and dissolve into a transparent solution, then weigh 1.5026g of thioacetamide and add it to the above transparent solution, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, pour the liquid into a polytetrafluoroethylene liner and seal it, then put the polytetrafluoroethylene liner into a stainless steel reactor and tighten it, and then place it in an oven at 160°C for 24 hours. After naturally cooling to room temperature, wash the obtained product with anhydrous ethanol and deoxygenated deionized water in turn; then put it in a refrigerator and freeze it for 12 hours, and then place it in a freeze dryer at -50°C for vacuum drying for 30 hours to obtain a molybdenum-doped vanadium disulfide precursor material;

[0068] 3) The third step is to perform P doping by heat treatment, wherein sodium hypophosphite is used as the P doping source, 0.4 g of sodium hypophosphite is placed in a magnetic boat at the center of the upstream heating zone of a tubular furnace, and a whole piece of the molybdenum-doped vanadium disulfide precursor material is placed in the magnetic boat and placed in the center of the downstream heating zone; in an argon atmosphere, the temperature of the upstream heating zone is controlled to be 300°C, and the temperature of the downstream heating zone is controlled to be 500°C, and the temperature is kept for 3 hours. After cooling to room temperature, a VS2 electrocatalytic electrode material co-doped with molybdenum cations and phosphorus anions is obtained.

[0069] X-ray diffractometer (XRD) was used to characterize the structure of the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material obtained above, as shown in FIG. Figure 1As shown, the results show that the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is a single vanadium disulfide phase without other impurity phases, and its 011 plane shifts to the left due to P doping; SEM is used to characterize the morphology of the above-mentioned molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material. The molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is self-assembled by nano-sheet molybdenum cation and phosphorus anion co-doped VS2 catalyst material to form a micron-sized flower-like structure uniformly grown on a carbon cloth substrate. EDS is used to perform surface scanning analysis on the above-mentioned molybdenum cation and phosphorus anion co-doped VS2 catalyst material. The results show that the material contains four elements, Mo, P, V, and S, and they are uniformly distributed.

[0070] The electrochemical hydrogen evolution performance of the molybdenum cation and phosphorus anion co-doped VS2 catalyst material was tested using a three-electrode system, with a carbon rod as the counter electrode, a Hg|Hg2SO4 electrode as the reference electrode, a molybdenum cation and phosphorus anion co-doped VS2 catalyst material as the working electrode, and a 0.5 mol / L sulfuric acid solution as the electrolyte. The test instrument was the Shanghai Chenhua CHI660E electrochemical workstation. The linear scan range of the linear scan voltammetry curve was between -1.0 and 0 V (relative to the standard hydrogen electrode), and the scan rate was 3 mV / s. All tests were performed in a constant temperature 25°C water bath environment. The test results are shown in Figure 2. Figure 5 and Figure 6 As shown, after data processing and calculation, at 50mAcm -2 The overpotential is as low as -0.2517V (relative to standard hydrogen electrode) and the Tafel slope is as low as 54.7mV / dec at the current density. The linear scanning range of the linear cyclic voltammetry curve is between 0.15 and 0.25V (relative to standard hydrogen electrode). Figure 8 As shown, it can be seen that the CV curves of all materials are rectangular in shape, indicating that no redox reaction occurs. Fig.12 The capacitive current density (Δj = j a -j b , where j a and j b It shows the relationship between the current density in the CV curve at 0.20V (relative to the standard hydrogen electrode) and the scan rate and its linear fitting function. Sample C dl The value is equal to half of the slope of the straight line in the figure, and its C dl The value is 75.9mF cm -2 .

[0071] Comparative Example 1:

[0072] 1) First step: Carbon cloth (CC) treatment: Cut the carbon cloth into rectangular pieces of 1 cm × 1.5 cm in size, soak the carbon cloth in a mixed acid of nitric acid and sulfuric acid in a ratio of 3:1 for more than 12 hours, then ultrasonically wash it with deionized water and anhydrous ethanol for more than three times, and then dry it in a vacuum drying oven at 60°C;

[0073] 2) The second step is to synthesize Mo-doped VS2 material, the preparation method of which is to weigh 0.2106g of ammonium metavanadate, 0.0353g of ammonium molybdate and 2ml of ammonia water, add them to water, stir and dissolve into a transparent solution, then weigh 1.5026g of thioacetamide and add it to the above transparent solution, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, pour the liquid into a polytetrafluoroethylene liner and seal it, then put the polytetrafluoroethylene liner into a stainless steel reactor and tighten it, and then place it in an oven at 160°C for 24 hours. After naturally cooling to room temperature, wash the obtained product with anhydrous ethanol and deoxygenated deionized water in turn; then put it in a refrigerator and freeze it for 12 hours, and then place it in a freeze dryer at -50°C for vacuum drying for 30 hours to obtain molybdenum-doped vanadium disulfide material;

[0074] X-ray diffractometer (XRD) was used to characterize the structure of the Mo-doped VS2 electrocatalytic electrode material obtained above. Figure 1 As shown, the results indicate that the Mo-doped VS2 electrocatalytic electrode material is a single vanadium disulfide phase without the presence of other impurity phases.

[0075] The electrochemical hydrogen evolution performance of Mo-doped VS2 catalyst material was tested using a three-electrode system, with a carbon rod as the counter electrode, a Hg|Hg2SO4 electrode as the reference electrode, a molybdenum-doped vanadium disulfide material as the working electrode, and a 0.5 mol / L sulfuric acid solution as the electrolyte. The test instrument was a Shanghai Chenhua CHI660E electrochemical workstation. The linear scanning range of the linear sweep voltammetric curve was between -1.0 and 0 V (relative to the standard hydrogen electrode), and the scanning speed was 3 mV / s. All tests were performed in a constant temperature 25°C water bath environment. The test results are shown in Figure 2. Figure 5 and Figure 6 As shown, after data processing and calculation, at 50 mA cm -2 The overpotential is as low as -0.2694V (relative to standard hydrogen electrode) and the Tafel slope is as low as 63.3mV / dec at the current density. The linear scanning range of the linear cyclic voltammetry curve is between 0.15 and 0.25V (relative to standard hydrogen electrode). Fig. 9 As shown, it can be seen that the CV curves of all materials are rectangular in shape, indicating that no redox reaction occurs. Fig.12 The capacitive current density (Δj = j a -j b , where j a and j bIt shows the relationship between the current density in the CV curve at 0.20V (relative to the standard hydrogen electrode) and the scan rate and its linear fitting function. Sample C dl The value is equal to half of the slope of the straight line in the figure, and its C dl The value is 62.5mF cm -2 .

[0076] Comparative Example 2:

[0077] 1) First step: Carbon cloth (CC) treatment: Cut the carbon cloth into rectangular pieces of 1 cm × 1.5 cm in size, soak the carbon cloth in a mixed acid of nitric acid and sulfuric acid in a ratio of 3:1 for more than 12 hours, then ultrasonically wash it with deionized water and anhydrous ethanol for more than three times, and then dry it in a vacuum drying oven at 60°C;

[0078] 2) The second step is to synthesize a pure VS2 precursor, the preparation method of which is to add a vanadium source and ammonia water into water, stir until transparent, then add a sulfur source, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, and then subject the mixed solution to a one-step hydrothermal reaction. The reaction product is washed and dried to obtain a pure vanadium disulfide precursor material;

[0079] The preparation method is to weigh 0.2106g of ammonium metavanadate, add 2ml of ammonia water to water, stir and dissolve into a transparent solution, then weigh 1.5026g of thioacetamide and add it to the above transparent solution, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, pour the liquid into a polytetrafluoroethylene liner and seal it, then put the polytetrafluoroethylene liner into a stainless steel reactor and tighten it, and then place it in a 160°C oven for 24 hours. After naturally cooling to room temperature, wash the obtained product with anhydrous ethanol and deoxygenated deionized water in turn; then put it in a refrigerator and freeze it for 12 hours, and then place it in a freeze dryer at -50°C for vacuum drying for 30 hours to obtain pure vanadium disulfide precursor material;

[0080] 3) The third step is to perform P doping by heat treatment. The preparation method is to use sodium hypophosphite as the P doping source, place 0.4g of sodium hypophosphite in a magnetic boat at the center of the upstream heating zone of the tubular furnace, place the above-mentioned whole piece of pure vanadium disulfide precursor material in the magnetic boat, and place it in the center of the downstream heating zone; in an argon atmosphere, heat and raise the temperature, control the temperature of the upstream heating zone to 300°C, the temperature of the downstream heating zone to 400°C, keep warm for 3 hours, cool to room temperature, and obtain a P-doped VS2 electrocatalytic electrode material.

[0081] X-ray diffractometer (XRD) was used to characterize the structure of the P-doped VS2 electrocatalytic electrode material obtained above. Figure 1 As shown, the results indicate that the molybdenum cation and phosphorus anion co-doped VS2 electrocatalytic electrode material is a single vanadium disulfide phase without the presence of other impurity phases, and the left shift of its 011 plane is caused by P doping.

[0082] The electrochemical hydrogen evolution performance of the P-doped VS2 electrocatalytic electrode material was tested using a three-electrode system, with a carbon rod as the counter electrode, a Hg|Hg2SO4 electrode as the reference electrode, a P-doped VS2 electrocatalytic electrode material as the working electrode, and a 0.5 mol / L sulfuric acid solution as the electrolyte. The test instrument was a Shanghai Chenhua CHI660E electrochemical workstation. The linear scan range of the linear scan voltammetric curve was between -1.0 and 0 V (relative to the standard hydrogen electrode), and the scan rate was 3 mV / s. All tests were performed in a constant temperature 25°C water bath environment. The test results are shown in Figure 2. Figure 5 and Figure 6 As shown, after data processing and calculation, at 50mAcm -2 The overpotential is as low as -0.2743V (relative to standard hydrogen electrode) and the Tafel slope is as low as 64.6mV / dec at the current density. The linear scanning range of the linear cyclic voltammetry curve is between 0.15 and 0.25V (relative to standard hydrogen electrode). Fig.10 As shown, it can be seen that the CV curves of all materials are rectangular in shape, indicating that no redox reaction occurs. Fig.12 The capacitive current density (Δj = j a -j b , where j a and j b It shows the relationship between the current density in the CV curve at 0.20V (relative to the standard hydrogen electrode) and the scan rate and its linear fitting function. Sample C dl The value is equal to half of the slope of the straight line in the figure, and its C dl The value is 60.3mFcm -2 .

[0083] Comparative Example 3:

[0084] 1) First step: Carbon cloth (CC) treatment: Cut the carbon cloth into rectangular pieces of 1 cm × 1.5 cm in size, soak the carbon cloth in a mixed acid of nitric acid and sulfuric acid in a ratio of 3:1 for more than 12 hours, then ultrasonically wash it with deionized water and anhydrous ethanol for more than three times, and then dry it in a vacuum drying oven at 60°C;

[0085] 2) The second step is to synthesize pure vanadium disulfide material, and the preparation method thereof is to add vanadium source and ammonia water into water, stir until transparent, then add sulfur source, stir to obtain a mixed solution; then add carbon cloth as a growth substrate, and then subject the mixed solution to a one-step hydrothermal reaction, and the reaction product is washed and dried to obtain pure vanadium disulfide material;

[0086] X-ray diffractometer (XRD) was used to characterize the structure of the pure vanadium disulfide material obtained above. Figure 1As shown, the results show that the pure vanadium disulfide material is a single vanadium disulfide phase without other impurity phases. The morphology of the above pure vanadium disulfide material was characterized by SEM, as shown in Fig.15 As shown in the figure, it can be seen that the pure vanadium disulfide material is self-assembled by nano-sheet pure vanadium disulfide material to form a micron-sized flower-like structure uniformly grown on the carbon cloth substrate. The pure vanadium disulfide material is subjected to surface scanning analysis using EDS, as shown in FIG. Fig.16 As shown, the results show that the material contains three elements, V and S, and they are evenly distributed.

[0087] The electrochemical hydrogen evolution performance of pure vanadium disulfide material was tested using a three-electrode system, with a carbon rod as the counter electrode, a Hg|Hg2SO4 electrode as the reference electrode, pure vanadium disulfide material as the working electrode, and a 0.5 mol / L sulfuric acid solution as the electrolyte. The test instrument was a Shanghai Chenhua CHI660E electrochemical workstation. The linear sweep voltammetric curve had a linear sweep range of -1.0 to 0 V (relative to the standard hydrogen electrode), a sweep speed of 3 mV / s, and all tests were performed in a constant temperature 25°C water bath environment. The test results are shown in Figure 2. Figure 5 and Figure 6 As shown, after data processing and calculation, at 50 mA cm -2 The overpotential is as low as -0.5514V (relative to standard hydrogen electrode) at the current density, and the Tafel slope is 209.7mV / dec. The linear scanning range of the linear cyclic voltammetry curve is between 0.15 and 0.25V (relative to standard hydrogen electrode). The results are as follows Fig.11 As shown, it can be seen that the CV curves of all materials are rectangular in shape, indicating that no redox reaction occurs. Fig.12 The capacitive current density (Δj = j a -j b , where j a and j b It shows the relationship between the current density in the CV curve at 0.20V (relative to the standard hydrogen electrode) and the scan rate and its linear fitting function. Sample C dl The value is equal to half of the slope of the straight line in the figure, and its C dl The value is 3.0mF cm -2 .

[0088] The above description is only a partial implementation mode of the present invention, and does not limit the present invention in any form. Any simple modification, change and modification made to the above implementation mode according to the technical essence of the present invention shall fall within the scope of the technical solution of the present invention.

Claims

1. A VS2 catalytic material co-doped with molybdenum cations and phosphorus anions, characterized in that: The micro-flowers are uniformly grown on a carbon-based material; the micro-flowers are assembled from VS2 nanosheets co-doped with molybdenum cations and phosphorus anions.

2. A VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to claim 1, characterized in that: In the co-doped VS2 of molybdenum cations and phosphorus anions, the doping amount of molybdenum cations is measured by the atomic ratio of Mo to V being (0.05-0.15):(0.95-0.85), and the doping amount of phosphorus anions is measured by the atomic ratio of P to S being (0.01-0.15):(0.99-0.85).

3. A VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to claim 1 or 2, characterized in that: The microflowers grow into a layered structure.

4. The VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to claim 1, characterized in that: The carbon-based material is carbon cloth.

5. The method for preparing a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to any one of claims 1 to 4, characterized in that: The following steps are involved: 1) performing oxidation pretreatment on the surface of the carbon-based material to obtain a pretreated carbon-based material; 2) adding a molybdenum source, a vanadium source and aqueous ammonia to water, stirring until transparent, and then adding a sulfur source and stirring to obtain a mixed solution; The mixed solution is transferred into a reactor containing a pretreated carbon-based material to undergo a hydrothermal reaction to obtain a molybdenum-doped vanadium disulfide material; 3) Using sodium hypophosphite as a phosphorus source, phosphorus-doping the molybdenum-doped vanadium disulfide material is performed through a heat treatment method to obtain the obtained material.

6. The method for preparing a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to claim 5, characterized in that: The oxidation pretreatment process is: soaking the carbon-based material in a mixed acid of nitric acid and sulfuric acid.

7. The method for preparing a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to claim 5, characterized in that: The molybdenum source includes at least one of ammonium molybdate, sodium molybdate and potassium molybdate; The vanadium source includes ammonium metavanadate and / or sodium vanadate; The sulfur source includes thiourea and / or thioacetamide; The molybdenum source, vanadium source and sulfur source are measured according to the atomic ratio of molybdenum, vanadium and sulfur of (0.05-0.15): (0.95-0.85): (5-10); the mass ratio of the phosphorus source to the molybdenum-doped vanadium disulfide material is 1.2-1.7:

1.

8. The method for preparing a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to claim 5, characterized in that: The conditions of the hydrothermal reaction are: temperature of 140-220° C. and time of 12-26 hours.

9. The method for preparing a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to claim 5, characterized in that: The process of phosphorus doping of molybdenum-doped vanadium disulfide material by heat treatment is as follows: sodium hypophosphite is placed in the upstream heating zone of the tubular furnace, and the molybdenum-doped vanadium disulfide material is placed in the downstream heating zone of the tubular furnace. An inert atmosphere is filled into the tubular furnace, and the temperature of the upstream heating zone is controlled at 300-350°C, and the temperature of the downstream heating zone is controlled at 300-500°C. After keeping warm for 2-4 hours, the mixture is cooled to room temperature.

10. The use of a VS2 catalytic material co-doped with molybdenum cations and phosphorus anions according to any one of claims 1 to 3, characterized in that: Applied to electrocatalytic hydrogen evolution reaction.

Citation Information

Patent Citations

  • Molybdenum doped vanadium disulfide micron flower material and preparation method and application thereof

    CN109939699A

Cited By

  • Modified carbon-based material electrocatalyst as well as preparation method and application thereof

    CN120519905A