Bifunctional catalyst electrode, preparation method and application of bifunctional catalyst electrode in urea purification and continuous electrolysis oxygen production

By forming a bifunctional catalytic electrode by the nickel-cobalt bimetallic Prussian blue-derived composite material doped with molybdate on the nickel foam, the efficient catalytic problem of urea oxidation and oxygen precipitation reaction is solved, and the continuous process of urea purification and electrolyzing oxygen production is realized. , reduces voltage demand and energy consumption, and improves resource recycling efficiency.

CN118910668APending Publication Date: 2024-11-08BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411251791.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The lack of dual-function catalyst electrodes suitable for urea oxidation and oxygen precipitation reactions in the prior art makes it difficult to achieve continuous processes of urea purification and electrolyzing oxygen production, and the slow anode reaction requires high voltage to increase costs.

Method used

Using a nickel-cobalt bimetallic Prussian blue-derived composite material doped with molybdate on the surface of the foam nickel, the bifunctional catalytic electrode NiCo-PBA-LDH@Mo/NF is formed through electrochemical activation, which is used for urea oxidation and oxygen precipitation reactions to achieve low High current density at electric potential.

Benefits of technology

The efficient catalysis of urea oxidation and oxygen precipitation reaction is achieved, and only 1.360V and 1.577V vs. RHE potentials are required to obtain a current density of 100mAcm-2, reducing process costs and energy consumption, and realizing urea purification and resource recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910668A_ABST
    Figure CN118910668A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of electro-catalysis application, and provides a bifunctional catalyst electrode, a preparation method and application of the bifunctional catalyst electrode in urea purification and continuous electrolysis oxygen production. The preparation method comprises the following steps: firstly, obtaining a molybdate-doped nickel-cobalt bimetallic Prussian blue derivative composite material on the surface of foamed nickel, and then performing electrochemical activation treatment and composite material reconstruction to form the bifunctional catalytic electrode NiCo-PBA-LDH (at) Mo / NF which can be simultaneously applied to urea purification and electrolytic oxygen production. The bifunctional catalytic electrode is applied to a continuous preparation process of urea purification and electrolysis oxygen production, and due to the fact that the bifunctional catalytic electrode has excellent urea oxidation and oxygen evolution catalytic activity, the current density of 100 mA cm <-2 > can be obtained only through the electric potential of 1.360 V vs.RHE and the electric potential of 1.577 V vs.RHE in the urea oxidation reaction and the oxygen evolution reaction respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrocatalytic applications, and in particular relates to a bifunctional catalyst electrode, a preparation method and applications thereof in urea purification and continuous electrolytic oxygen production. Background Art

[0002] Domestic sewage and industrial wastewater from urea production contain a large amount of urea, which is a potential pollutant to the environment. Urea will naturally hydrolyze to produce unstable ammonia, which will then be oxidized into pollutants such as nitrates, nitrites, and nitrogen oxides; it will also cause eutrophication of water bodies, resulting in the proliferation of algae, reduced oxygen-rich water bodies, and fish deaths. Therefore, excessive urea will pollute the air, soil, and water. On the other hand, through urea electrolysis, urea can be decomposed into harmless nitrogen and water, reducing the pollution of excessive urea to the environment. At the same time, urea electrolysis can also obtain clean energy hydrogen. In addition, the water after urea purification can continue to be powered on, and oxygen and hydrogen production can continue to be achieved through water electrolysis. This achieves the purification of urea wastewater and the recycling of resources.

[0003] Whether it is urea electrolysis or water electrolysis after wastewater purification, the anode of both will cause the reaction to proceed slowly due to the multi-electron transfer process, which requires a higher voltage, resulting in increased costs and is not conducive to the application and promotion of technology. In order to solve this problem, it is usually necessary to use an electrocatalyst to speed up the reaction process. In the prior art, there is no catalyst electrode that is suitable for both urea oxidation reaction and oxygen evolution reaction, so it is impossible to achieve a continuous process of urea purification and water electrolysis oxygen production. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention proposes a bifunctional catalyst electrode, a preparation method and its application in urea purification and continuous electrolytic oxygen production. First, a molybdate-doped nickel-cobalt bimetallic Prussian blue-derived composite material is obtained on the surface of nickel foam. Then, after electrochemical activation treatment, the composite material is reconstructed to form a bifunctional catalytic electrode NiCo-PBA-LDH@Mo / NF that can be simultaneously used for urea oxidation and oxygen evolution reactions. The bifunctional catalytic electrode is applied to the continuous preparation process of urea electrolysis and oxygen evolution. Since the bifunctional catalytic electrode has excellent catalytic activity for urea oxidation and oxygen evolution, only 1.360V vs.RHE and 1.577V vs.RHE potentials are required for urea oxidation and oxygen evolution reactions, respectively, to obtain 100mAcm -2 of current density.

[0005] The specific technical solutions of the present invention are as follows:

[0006] A method for preparing a bifunctional catalyst electrode comprises the following steps:

[0007] Step S1: synthesizing a precursor PBA having a cubic nanostructure based on a deionized aqueous solution of nickel chloride, sodium citrate dihydrate and potassium hexacyanocobaltate, and obtaining the precursor PBA by centrifugation, washing and drying;

[0008] Step S2: pre-treating the nickel foam by deoxidizing, rinsing and drying the nickel foam;

[0009] Step S3: synthesizing a catalyst electrode, fully dissolving molybdenum trioxide and sodium citrate dihydrate in deionized water, adding a precursor PBA, ultrasonically obtaining a blue suspension, adding a pretreated nickel foam, and performing a one-step hydrothermal reaction, rinsing and drying the reaction product to obtain a nickel foam composite material having a cubic structure of molybdate-doped Prussian blue derivatives on the surface, and processing the composite material into a catalyst electrode NiCo-PBA-LDH@Mo / NF;

[0010] Step S4: activating the catalyst electrode, and forming a molybdate-doped nickel-cobalt double-layer hydroxide on the surface of the catalyst electrode through multiple cyclic voltammetry scans to obtain a bifunctional catalyst electrode.

[0011] Preferably, the step S1 specifically includes:

[0012] Step S11: dissolving nickel chloride and sodium citrate dihydrate in deionized water;

[0013] Step S12: dissolving potassium hexacyanocobaltate in deionized water;

[0014] Step S13: mixing the two solutions obtained in step S11 and step S12, stirring them thoroughly and leaving them to stand at room temperature for 24 hours;

[0015] Step S14: The mixed solution obtained in step S13 is centrifuged and washed multiple times to obtain a precipitate, which is then dried at 60° C. to obtain a precursor PBA.

[0016] Preferably, the amount of deionized water in step S11 and step S12 is the same.

[0017] Preferably, in step S11, the mass ratio of nickel chloride to sodium citrate dihydrate is 2:3.

[0018] Preferably, the step S2 specifically includes:

[0019] Step S21: Cut the nickel foam into 2 cm 2 size;

[0020] Step S22: placing the nickel foam in dilute hydrochloric acid for ultrasonic treatment to remove the oxide layer of the nickel foam;

[0021] Step S23: Rinse with deionized water and ethanol until neutral, and dry at room temperature for later use.

[0022] Preferably, the step S3 specifically includes:

[0023] Step S31: dissolving molybdenum trioxide and sodium citrate dihydrate in deionized water, and stirring thoroughly until the solution is clear;

[0024] Step S32: dispersing the precursor PBA in the solution obtained in step S31, and obtaining a uniform suspension by ultrasonication and sufficient stirring;

[0025] Step S33: transferring the uniform suspension to a hydrothermal kettle, and adding the nickel foam pretreated in step S2;

[0026] Step S34: After the hydrothermal autoclave is maintained at 180° C. for 10 hours, the obtained product is repeatedly rinsed with deionized water and ethanol, and dried to obtain a foam nickel composite material having a cubic structure of molybdate-doped Prussian blue derivatives on the surface;

[0027] Step S35: Processing the composite material into a catalyst electrode NiCo-PBA-LDH@Mo / NF.

[0028] Preferably, the mass ratio of molybdenum trioxide to sodium citrate dihydrate in step S31 is 2:3.

[0029] Preferably, the process parameters of the cyclic voltammetry scan in step S4 are as follows: a scan rate of 200 mV / s, a potential range of 0.15-0.8 V, and a scan speed of 30 cycles.

[0030] A bifunctional catalyst electrode is obtained by the above-mentioned preparation method, wherein the NiCo-PBA-LDH@Mo / NF is composed of molybdate-doped nickel-cobalt layered double hydroxide.

[0031] An application of a bifunctional catalyst electrode, wherein the bifunctional catalyst electrode is used for urea purification and continuous electrolytic oxygen production, comprising the following steps:

[0032] Step 1: using the bifunctional catalyst electrode as an anode to carry out urea oxidation reaction;

[0033] Step 2: After the urea is completely purified, the current is maintained unchanged, and the electrolysis potential is raised to the potential required for the oxygen evolution reaction to carry out the oxygen evolution reaction, thereby obtaining hydrogen and oxygen.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The present invention proposes a bifunctional catalyst electrode capable of taking into account both urea oxidation and oxygen evolution and a preparation method thereof. The bifunctional catalyst electrode has excellent catalytic activity for urea oxidation and oxygen evolution, and when used for urea oxidation, only a potential of 1.360 V vs. RHE is required to obtain 100 mA cm -2 For oxygen evolution reaction, only 1.577 V vs. RHE is required to obtain 100 mA cm -2 of current density.

[0036] 2. The bifunctional catalyst electrode preparation method proposed in the present invention is prepared by hydrothermal method at a relatively low temperature, with low energy consumption, easy control, low raw material cost and simple preparation method.

[0037] 3. The present invention proposes an application of a bifunctional catalyst electrode, which can achieve one-step purification of urine urea and subsequent electrolysis of water to produce oxygen through electrolysis reaction. At the same time, hydrogen evolution reaction occurs in the cathode half reaction of the two reactions to produce hydrogen, thereby achieving the purpose of resource utilization of human waste. The electrolysis process is simple and can be achieved using the mature automatic control program of the electrochemical workstation. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. The features and advantages of the present invention can be more clearly understood by referring to the drawings. The drawings are schematic and should not be understood as limiting the present invention in any way. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0039] Figure 1 The present invention is a flow chart of a method for preparing a bifunctional catalyst electrode.

[0040] Figure 2 This is the SEM picture of the catalyst electrode NiCo-PBA-LDH@Mo / NF before activation in Example 1.

[0041] Figure 3 This is the SEM image of the catalyst electrode NiCo-PBA-LDH@Mo / NF after activation in Example 1.

[0042] Figure 4 This is a SEM image of the bifunctional catalyst electrode in Example 1 after reacting in a urea-containing solution for 10 minutes.

[0043] Figure 5 This is the HRTEM lattice image obtained by ultrasound after activation of the catalyst electrode NiCo-PBA-LDH@Mo / NF in Example 1.

[0044] Figure 6 This is the linear voltammetric scan curve of the bifunctional catalyst electrode in simulated urine and alkaline water.

[0045] Figure 7 This is a graph showing the chronopotentiometry test of the bifunctional catalyst electrode in simulated urine.

[0046] Figure 8 The liquid chromatograms of simulated urine and simulated urine after electrolysis for 10, 25, and 45 hours. DETAILED DESCRIPTION

[0047] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0048] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0049] Example 1

[0050] 1. Preparation of bifunctional catalyst electrodes, such as Figure 1 shown.

[0051] Step S1: Synthesis of precursor PBA with cubic nanostructure:

[0052] (1) dissolving 0.36 mmol of nickel chloride and 0.54 mmol of sodium citrate dihydrate in 20 mL of deionized water, wherein the mass ratio of nickel chloride to sodium citrate dihydrate is 2:3;

[0053] (2) Dissolve 0.48 mmol potassium hexacyanocobaltate in 20 mL deionized water;

[0054] (3) mixing the two solutions, stirring them thoroughly and leaving them to stand at room temperature for 24 hours;

[0055] (4) The precipitate is obtained by multiple centrifugal washing, and the precipitate is dried in an oven at 60° C. to obtain the precursor PBA.

[0056] Step S2: Pretreatment of nickel foam: Cut the nickel foam into 1×2 cm 2 The size of the nickel foam was placed in 3M dilute hydrochloric acid and ultrasonicated for 20 minutes to remove the oxide layer of the nickel foam, and then rinsed with deionized water and ethanol until neutral. After rinsing, it was dried at room temperature for use.

[0057] Step S3: Synthesis of catalyst electrode:

[0058] (1) Dissolve 1.08 mmol of molybdenum trioxide and 1.62 mmol of sodium citrate dihydrate in 40 mL of deionized water, wherein the mass ratio of molybdenum trioxide to sodium citrate dihydrate is 2:3, and stir thoroughly until the solution is clear;

[0059] (2) 80 mg of the precursor PBA was dispersed in the clear solution, and a uniform suspension was formed by ultrasonic treatment for 5 min and stirring for 30 min;

[0060] (3) Transfer the uniform suspension to a 50 mL hydrothermal kettle and then add the pretreated nickel foam;

[0061] (4) After the hydrothermal autoclave is kept at 180° C. for 10 h, the obtained product is repeatedly rinsed with deionized water and ethanol, and dried at 60° C. to obtain a foam nickel composite material having a cubic structure of molybdate-doped Prussian blue derivatives on the surface;

[0062] (5) Process the composite material into catalyst electrode NiCo-PBA-LDH@Mo / NF.

[0063] Step S4: Activate the catalyst electrode: perform multiple cyclic voltammetry scans, wherein the scan rate is 200 mV / s, the potential range is 0.15-0.8 V, and the scan circle speed is 30 circles, thereby forming a molybdate-doped nickel-cobalt double-layer hydroxide on the surface of the catalyst electrode to obtain a bifunctional catalyst electrode.

[0064] Scanning electron microscope (JSM 6010, JEOL, Japan) was used to observe the morphology of the catalyst electrode NiCo-PBA-LDH@Mo / NF in Example 1 before and after activation and after the bifunctional catalyst electrode catalyzed urea oxidation reaction in a urea-containing solution for 10 minutes. The morphology of the catalyst electrode NiCo-PBA-LDH@Mo / NF before activation is as follows: Figure 2 As shown in the figure, it can be observed that dense cubic particles are formed on the substrate nickel foam, while the surface of the nickel foam itself is smooth. Figure 3 As shown in the figure, after electrochemical activation treatment, the cubic particles change from smooth to rough, and small particles are attached to the surface of nickel foam. Figure 4 As shown, after urea oxidation reaction in urea-containing solution for 10 min, the cubes decomposed into spherical particles and grew on the surface of nickel foam.

[0065] Transmission electron microscopy (JEM-2100F, JEOL, Japan) was used to observe the catalyst electrode NiCo-PBA-LDH@Mo / NF sample obtained after activation and ultrasonic treatment. Figure 5The lattice spacings of 0.239 and 0.260 nm correspond to the (104) and (012) planes of NiCo-LDH, the lattice spacing of 0.271 nm corresponds to the (110) plane of Ni(OH)2, and the lattice spacing of 0.218 nm corresponds to the (110) plane of CoOOH.

[0066] 2. Electrolysis performance test and urea consumption test of bifunctional catalyst electrode

[0067] Electrochemical workstation CHI 760e (CH instrument, Shanghai, China) was used for electrolysis test. Human urine contains about 2-2.5% urea by mass. Considering the application of treating urea in urine, an alkaline aqueous solution with a urea molar concentration of 0.33 mol / L was prepared as simulated urine. Figure 6 As shown in the figure, the bifunctional catalyst electrode was first used to perform linear voltammetric scanning tests in simulated urine and alkaline water. According to the curve, it can be concluded that the bifunctional catalyst electrode only needs a potential of 1.360V vs. RHE to obtain 100mAcm when urea oxidation reaction occurs in simulated urine. -2 When the electrolysis of water and oxygen evolution occurs in alkaline water, only a potential of 1.577 V vs. RHE is required to obtain 100 mA cm -2 The current density of the two reactions is 100 mA cm -2 The potential difference at the current density is 0.217V.

[0068] The urea electrolysis purification test was performed using the chronopotentiometry (CP) method of the electrochemical workstation. The current passing through the circuit was fixed at 0.1A, and 40mL of simulated urine was quantitatively taken for electrolysis. Since the potential required for the urea oxidation reaction is lower than that for the oxygen evolution reaction, during the electrolysis process, in order to maintain the current unchanged, the required potential will gradually increase as the urea is consumed by electrolysis. The applied potential can be automatically controlled by the electrochemical workstation program to rise to the potential of oxygen evolution, achieving continuous electrolysis. Figure 7As shown, the test curve can be roughly divided into three parts: the first section is about the first 7.5 hours, when urea oxidation reaction occurs to purify urea; the second section is about 7.5-16 hours, which is a transition section. In this section, due to the decrease in urea concentration in the solution, competition between urea oxidation reaction and oxygen evolution reaction from water electrolysis will occur, and the potential value will continue to oscillate between the potential values ​​corresponding to the two reactions. Affected by diffusion, when the urea concentration around the surface of the bifunctional catalyst electrode is too low to cover all the catalyst active sites, the potential value increases and oxygen evolution reaction occurs. When urea in the liquid diffuses to the vicinity of the bifunctional catalyst electrode, causing the local concentration to increase, the bifunctional catalyst electrode again preferentially catalyzes urea oxidation, and the potential value drops to the corresponding value of the urea oxidation reaction; the third section is about 16 hours later, when the urea in the entire solution is basically consumed, oxygen evolution reaction from water electrolysis occurs on the bifunctional catalyst electrode. The potential rise in the second section is about 0.2V, which is in line with Figure 6 Simulated urine electrolysis and water electrolysis oxygen production at 100 mA cm -2 The voltage conversion value at , proves that the conversion of urine electrolysis to water electrolysis has occurred.

[0069] The urea content in the simulated urine and the simulated urine after 10, 25, and 45 hours of electrolysis was tested using a high performance liquid chromatograph (Agilent 1200, Agilent). Figure 8 As shown, the characteristic peak of urea measured in the original simulated urine in (a) appears at 4.472 min; in (b) and (c), the characteristic peak of urea in the solution after 10 and 25 hours of electrolysis is significantly weakened, proving that the urea in the solution has indeed been purified; in (d), the characteristic peak of urea in the solution after 45 hours of electrolysis basically disappears, proving that the urea in the solution has been purified.

[0070] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0071] In the present invention, the terms "first", "second", "third", "fourth" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance. The term "plurality" refers to two or more, unless otherwise clearly defined.

[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a bifunctional catalyst electrode, characterized in that: The following steps are involved: Step S1: synthesizing a precursor PBA having a cubic nanostructure, based on a deionized aqueous solution of nickel chloride, sodium citrate dihydrate and potassium hexacyanocobaltate, and obtaining the precursor PBA by centrifugation, washing and drying; Step S2: pre-treating the nickel foam by deoxidizing, rinsing and drying the nickel foam; Step S3: synthesizing a catalyst electrode, fully dissolving molybdenum trioxide and sodium citrate dihydrate in deionized water, adding a precursor PBA, ultrasonically obtaining a blue suspension, adding a pretreated nickel foam, and performing a one-step hydrothermal reaction, rinsing and drying the reaction product to obtain a nickel foam composite material having a cubic structure of molybdate-doped Prussian blue derivatives on the surface, and processing the composite material into a catalyst electrode NiCo-PBA-LDH@Mo / NF; Step S4: activating the catalyst electrode, and forming a molybdate-doped nickel-cobalt double-layer hydroxide on the surface of the catalyst electrode through multiple cyclic voltammetry scans to obtain a bifunctional catalyst electrode.

2. The method for preparing a bifunctional catalyst electrode according to claim 1, characterized in that: The step S1 specifically includes: Step S11: dissolving nickel chloride and sodium citrate dihydrate in deionized water; Step S12: dissolving potassium hexacyanocobaltate in deionized water; Step S13: mixing the two solutions obtained in step S11 and step S12, stirring them thoroughly and leaving them to stand at room temperature for 24 hours; Step S14: The mixed solution obtained in step S13 is centrifuged and washed multiple times to obtain a precipitate, which is then dried at 60° C. to obtain a precursor PBA.

3. The method for preparing a bifunctional catalyst electrode according to claim 2, characterized in that: The amount of deionized water in step S11 and step S12 is the same.

4. The method for preparing a bifunctional catalyst electrode according to claim 2, characterized in that: In the step S11, the mass ratio of nickel chloride to sodium citrate dihydrate is 2:

3.

5. The method for preparing a bifunctional catalyst electrode according to claim 1, characterized in that: The step S2 specifically includes: Step S21: Cut the nickel foam into 2 cm 2 size; Step S22: placing the nickel foam in dilute hydrochloric acid for ultrasonic treatment to remove the oxide layer of the nickel foam; Step S23: Rinse with deionized water and ethanol until neutral, and dry at room temperature for later use.

6. The method for preparing a bifunctional catalyst electrode according to claim 1, characterized in that: The step S3 specifically includes: Step S31: dissolving molybdenum trioxide and sodium citrate dihydrate in deionized water, and stirring thoroughly until the solution is clear; Step S32: dispersing the precursor PBA in the solution obtained in step S31, and obtaining a uniform suspension by ultrasonication and sufficient stirring; Step S33: transferring the uniform suspension to a hydrothermal kettle, and adding the nickel foam pretreated in step S2; Step S34: After the hydrothermal autoclave is maintained at 180° C. for 10 hours, the obtained product is repeatedly rinsed with deionized water and ethanol, and dried to obtain a foam nickel composite material having a cubic structure of molybdate-doped Prussian blue derivatives on the surface; Step S35: Processing the composite material into a catalyst electrode NiCo-PBA-LDH@Mo / NF.

7. The method for preparing a bifunctional catalyst electrode according to claim 6, characterized in that: The mass ratio of molybdenum trioxide to sodium citrate dihydrate in step S31 is 2:

3.

8. The method for preparing a bifunctional catalyst electrode according to claim 1, characterized in that: The process parameters of the cyclic voltammetry scan in step S4 are as follows: the scan rate is 200 mV / s, the potential range is 0.15-0.8 V, and the scan circle speed is 30 circles.

9. A bifunctional catalyst electrode, characterized in that: The NiCo-PBA-LDH@Mo / NF is obtained by the preparation method according to any one of claims 1 to 8, and is composed of molybdate-doped nickel-cobalt layered double hydroxide.

10. An application of the bifunctional catalyst electrode as claimed in claim 9, wherein the bifunctional catalyst electrode is used for urea purification and continuous electrolytic oxygen production, comprising the following steps: Step 1: using the bifunctional catalyst electrode as an anode to carry out urea oxidation reaction; Step 2: After the urea is completely purified, the current is maintained unchanged, and the electrolysis potential is raised to the potential required for the oxygen evolution reaction to carry out the oxygen evolution reaction, thereby obtaining hydrogen and oxygen.