Production process of oxidation-resistant electrolytic copper foil

By forming a dense protective layer on the surface of the electrolytic copper foil and using specific electrolytic aids and antioxidants, the problem of insufficient oxidation resistance of the electrolytic copper foil is solved, extending the service life and improving the grade.

CN118910682APending Publication Date: 2024-11-08GUANGDONG FINE YUAN SCI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410962277.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing electrolytic copper foils have insufficient oxidation resistance, resulting in a shortened service life and a reduced quality.

Method used

Using an oxidation-resistant electrolytic copper foil production process, by forming a dense protective layer on the surface of the electrolytic copper foil, electrolyzing in the copper sulfate solution using specific electrolytic aids and antioxidants, combined with 2-mercaptobenzooxazole in the protective liquid Azoles and antioxidants form an oxidation-resistant protective layer, improving the antioxidant properties of electrolytic copper foil.

Benefits of technology

It effectively extends the service life of electrolytic copper foil, improves its grade, and maintains excellent mechanical properties and gloss, ensuring the quality of electrolytic copper foil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004950627150000031
    Figure BDA0004950627150000031
  • Figure BDA0004950627150000061
    Figure BDA0004950627150000061
  • Figure BDA0004950627150000081
    Figure BDA0004950627150000081
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic copper foil preparation, in particular to a production process of oxidation-resistant electrolytic copper foil. The preparation method comprises the following steps: carrying out nucleophilic addition reaction on a compound and ethyl 2-butynoate under the action of a reaction accelerator, then carrying out ester exchange reaction on a product component and hexadecanol under the action of dibutyltin oxide, after the reaction is finished, adjusting the pH value of a reaction product to 7.8-8.5, and carrying out suction filtration, washing and reduced pressure distillation to obtain an antioxidant finished product. Molecules of the prepared antioxidant contain two functional groups with an anti-oxidation function, the antioxidant has excellent anti-oxidation performance, the antioxidant and 2-mercaptobenzoxazole are jointly used as raw materials of a protective solution, the antioxidant and 2-mercaptobenzoxazole interact and cooperate with each other to form a compact protective layer on the surface of the electrolytic copper foil, the oxidation resistance of the electrolytic copper foil is effectively improved, and the service life of the electrolytic copper foil is prolonged. The oxidation rate of the electrolytic copper foil is delayed to a certain extent, the service life of the electrolytic copper foil is prolonged, and the grade of the electrolytic copper foil is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytic copper foil preparation, and in particular to a production process of oxidation-resistant electrolytic copper foil. Background Art

[0002] Electrolytic copper foil is a copper foil material prepared by electrolysis. It is made by immersing a copper plate in an electrolyte, then applying an electric current to cause copper ions to precipitate on the anode and deposit on the cathode to form copper foil. Electrolytic copper foil has high purity, uniform thickness and good conductivity, and is widely used in electronics, communications, semiconductors and other fields. It is often used to manufacture circuit boards, electronic components, solar cells, etc. In today's rapid development of the electronic information industry, electrolytic copper foil is called the "neural network" for signal and power transmission and communication of electronic products. The preparation process of electrolytic copper foil is precise and rigorous, and the thickness and surface quality of the foil can be controlled, so it has important application value in high-precision electronic products.

[0003] In the patent document with application number "CN201810953256.2" and titled "Additives for electrolytic copper foil and production process of 5-micron electrolytic copper foil for dual-light lithium battery", an additive for electrolytic copper foil and a production process of 5-micron electrolytic copper foil for dual-light lithium battery are disclosed. Although the electrolytic copper foil produced by this patent document has good brightness and tensile strength, its own oxidation resistance is relatively insufficient and it is easily oxidized, which shortens the service life of the electrolytic copper foil to a certain extent and reduces its quality. Therefore, the present invention provides a production process for oxidation-resistant electrolytic copper foil to solve this technical problem! Summary of the invention

[0004] The purpose of the present invention is to provide a production process of oxidation-resistant electrolytic copper foil. The produced electrolytic copper foil not only has excellent mechanical properties, but also has excellent antioxidant properties, which prolongs its service life to a certain extent, effectively ensures the quality of the electrolytic copper foil and also improves its grade.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A production process for oxidation-resistant electrolytic copper foil comprises the following steps:

[0007] Step 1: Put a high-purity copper wire with a purity of ≥99.97% into a sulfuric acid solution and heat it to dissolve it to obtain a copper sulfate solution; then add an electrolytic aid to the obtained copper sulfate solution, mix it evenly, and then transport the obtained electrolyte to an electrolytic cell and perform electrolysis at a temperature of 50-60°C; the obtained electrolytic copper foil is stored and used for standby; wherein, the copper in the copper sulfate solution is 2+ The concentration is 90~95g / L, SO4 2- The concentration is 100-110 g / L;

[0008] Step 2: The electrolytic copper foil prepared in step 1 is transferred into a pickling tank for cleaning to remove the oxide film on the surface. The electrolytic copper foil is washed with water and then placed into a protective liquid and immersed at a temperature of 50 to 60° C. for 5 to 10 minutes to form an oxidation-resistant protective layer on the surface of the electrolytic copper foil.

[0009] Step 3: Take out the electrolytic copper foil treated in step 2 from the protective liquid and wash the protective liquid remaining on its surface with ethanol, then dry the electrolytic copper foil; after drying, cut, slit and package it, and finally obtain the finished oxidation-resistant electrolytic copper foil.

[0010] Furthermore, the electrolysis aid includes graphene oxide, gelatin, cerium sulfate, sodium chloride, cellulose hydroxypropyl methyl ether, a filler, polyethylene glycol, a brightener and polyethyleneimine.

[0011] Furthermore, the concentrations of the raw materials in the electrolytic aid in the electrolyte are as follows: graphene oxide: 3-6 mg / L, gelatin: 12-15 mg / L, cerium sulfate: 35-45 mg / L, sodium chloride: 20-25 mg / L, cellulose hydroxypropyl methyl ether: 5-8 mg / L, filler: 10-15 mg / L, polyethylene glycol: 6-10 mg / L, brightener: 20-40 mg / L, polyethylene imine: 35-40 mg / L; wherein the molecular weight of polyethylene imine is 1000-3000, and the number average molecular weight of gelatin is 1000-5000.

[0012] Furthermore, the current intensity during the electrolysis process is 20000-30000A, and the flow rate of the electrolyte is 45-50m 3 / h.

[0013] Furthermore, the leveling agent is selected from any one of sodium mercaptoimidazole propanesulfonate, tetrahydrothiazolidinethione, and ethylenethiourea.

[0014] Furthermore, the brightener is selected from any one of sodium polydisulfide propane sulfonate, sodium phenyl polydisulfide propane sulfonate, and sodium 3-mercapto-1-propane sulfonate.

[0015] Furthermore, the preparation method of the protective liquid is: 2-mercaptobenzoxazole, antioxidant, ethylene glycol, silane coupling agent, triethanolamine and dodecylethoxysulfobetaine are respectively mixed uniformly with an ethanol aqueous solution with a concentration of 30-40% to obtain the protective liquid; wherein the concentration of 2-mercaptobenzoxazole in the protective liquid is 0.5-0.8 g / L, the concentration of the antioxidant is 0.8-1.2 g / L, the concentration of ethylene glycol is 1.5-2.0 ml / L, the concentration of the silane coupling agent is 1.5-3.0 ml / L, the concentration of triethanolamine is 2-3 ml / L, and the concentration of dodecylethoxysulfobetaine is 3-5 g / L.

[0016] Furthermore, the silane coupling agent is selected from any one of vinyltriethoxysilane, vinyltrimethoxysilane and vinyltri(2-methoxyethoxy)silane.

[0017] Furthermore, the preparation method of the antioxidant comprises the following steps:

[0018] S1, putting the compound into acetonitrile with a mass of 5 to 8 times that of the compound, and sequentially adding 2-butynoic acid ethyl ester with a molar amount of 0.8 to 1.2 times that of the compound and a reaction accelerator with a molar amount of 0.2 to 0.4 times that of the compound, stirring and mixing evenly, introducing nitrogen, and raising the temperature of the mixed solution to 60 to 75° C. under the protection of nitrogen, stirring and reacting at this temperature for 10 to 15 hours; after the reaction is completed, naturally cooling the resultant components to room temperature, and then filtering and washing the resultant components with water and evaporating to remove the acetonitrile therein, and storing the obtained liquid product for standby use;

[0019] S2, putting the liquid product into a reaction device, and adding palm alcohol with a mass of 0.5 to 0.8 times that of the liquid product and xylene with a mass of 2 to 4 times that of the liquid product in sequence, stirring and introducing nitrogen to drive out the air in the reaction device, stirring and heating to 90 to 110° C., and then adding dibutyltin oxide with a mass of 0.03 to 0.05 times that of the palm alcohol, and keeping the temperature for reaction for 10 to 20 hours; after the reaction is completed, adjusting the pH of the reaction product to 7.8 to 8.5, and then filtering, washing and distilling under reduced pressure to obtain a liquid component is an antioxidant;

[0020] The structure of the compound is as follows:

[0021]

[0022] Furthermore, the reaction accelerator is selected from any one of triethylamine, aluminum trichloride and boron trifluoride.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] In the present invention, the compound is first put into acetonitrile, and 2-butynoic acid ethyl ester is added thereto, and the compound and 2-butynoic acid ethyl ester undergo nucleophilic addition reaction under the action of a reaction accelerator, after the reaction is completed, the resultant components are naturally cooled to room temperature, and then filtered and washed with water to remove the acetonitrile therein, and the obtained liquid product is put into a reaction device, and palmityl alcohol and xylene are added thereto, and after mixing and stirring evenly, the liquid product and palmityl alcohol undergo ester exchange reaction under the action of dibutyltin oxide, after the reaction is completed, the pH of the reaction product is adjusted to 7.8-8.5, and then filtered, washed and distilled under reduced pressure to obtain an antioxidant finished product. The prepared antioxidant molecule contains two functional groups with antioxidant function, has excellent antioxidant performance, and the antioxidant and 2-mercaptobenzoxazole are used as raw materials of protective liquid together, and the two interact with each other and cooperate with each other to form a dense protective layer on the surface of the electrolytic copper foil, which effectively improves the oxidation resistance of the electrolytic copper foil, slows down the oxidation rate of the electrolytic copper foil to a certain extent, and prolongs its service life. In addition, the electrolytic copper foil produced by the present invention also has excellent glossiness and mechanical properties, which effectively ensures its quality and improves its grade. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] A production process for oxidation-resistant electrolytic copper foil comprises the following steps:

[0028] Step 1: Put a high-purity copper wire with a purity of ≥99.97% into a sulfuric acid solution and heat it to dissolve it to obtain a copper sulfate solution; then add an electrolytic aid to the obtained copper sulfate solution, mix it evenly, and then transport the obtained electrolyte to an electrolytic cell and electrolyze it at a temperature of 50°C; the obtained electrolytic copper foil is stored and used for standby; wherein, the copper in the copper sulfate solution is 2+ The concentration is 90g / L, SO4 2- The concentration is 100g / L; the current intensity during electrolysis is 20000A, and the flow rate of the electrolyte is 45m 3 / h;

[0029] Step 2: The electrolytic copper foil prepared in step 1 is transferred into a pickling tank for cleaning to remove the oxide film on the surface. The electrolytic copper foil is washed with water and then placed into a protective liquid and immersed at a temperature of 50° C. for 5 minutes to form an oxidation-resistant protective layer on the surface of the electrolytic copper foil.

[0030] Step 3: Take out the electrolytic copper foil treated in step 2 from the protective liquid and wash the protective liquid remaining on its surface with ethanol, then dry the electrolytic copper foil; after drying, cut, slit and package it, and finally obtain the finished oxidation-resistant electrolytic copper foil.

[0031] The electrolytic aids include graphene oxide, gelatin, cerium sulfate, sodium chloride, cellulose hydroxypropyl methyl ether, sodium mercaptoimidazolepropanesulfonate, polyethylene glycol, sodium polydisulfide propanesulfonate and polyethyleneimine.

[0032] The specific concentrations of the raw materials in the electrolytic aid in the electrolyte are as follows: graphene oxide: 3 mg / L, gelatin: 12 mg / L, cerium sulfate: 35 mg / L, sodium chloride: 20 mg / L, cellulose hydroxypropyl methyl ether: 5 mg / L, sodium mercaptoimidazolepropanesulfonate: 10 mg / L, polyethylene glycol: 6 mg / L, sodium polydisulfide propanesulfonate: 20 mg / L, polyethyleneimine: 35 mg / L; wherein the molecular weight of polyethyleneimine is 1000, and the number average molecular weight of gelatin is 1000.

[0033] The preparation method of the protective liquid comprises the following steps: respectively mixing 2-mercaptobenzoxazole, an antioxidant, ethylene glycol, vinyl triethoxysilane, triethanolamine and dodecyl ethoxy sulfobetaine with a 30% ethanol aqueous solution and then uniformly preparing the protective liquid; wherein the concentration of 2-mercaptobenzoxazole in the protective liquid is 0.5 g / L, the concentration of the antioxidant is 0.8 g / L, the concentration of ethylene glycol is 1.5 ml / L, the concentration of vinyl triethoxysilane is 1.5 ml / L, the concentration of triethanolamine is 2 ml / L, and the concentration of dodecyl ethoxy sulfobetaine is 3 g / L.

[0034] The preparation method of the antioxidant comprises the following steps:

[0035] S1, put the compound into acetonitrile with a mass 5 times that of the compound, and add 2-butynoic acid ethyl ester and triethylamine with a molar amount of 0.8 times that of the compound in sequence, mix and stir evenly, then introduce nitrogen, and raise the temperature of the mixed solution to 60°C under the protection of nitrogen, and stir and react at this temperature for 10 hours; after the reaction is completed, cool the resultant components naturally to room temperature, then filter and wash the resultant components with water and evaporate the acetonitrile therein, and store the obtained liquid product for standby use;

[0036] S2, putting the liquid product into a reaction device, and adding 0.5 times the mass of palmityl alcohol and 2 times the mass of xylene of the liquid product in sequence, mixing and stirring evenly, introducing nitrogen to drive out the air in the reaction device, stirring and heating to 90°C, and then adding 0.03 times the mass of palmityl alcohol dibutyltin oxide thereto, and keeping the temperature for reaction for 10 hours; after the reaction is completed, adjusting the pH of the reaction product to 7.8, and then filtering, washing and distilling under reduced pressure to obtain a liquid component is an antioxidant;

[0037] The structure of the compound is as follows:

[0038]

[0039] Example 2

[0040] The production process of an oxidation-resistant electrolytic copper foil provided in this embodiment is basically the same as that in Embodiment 1, except that the specific composition of the electrolytic auxiliary agent and the preparation method of the antioxidant used are not exactly the same. The specific composition of the electrolytic auxiliary agent and the preparation method of the antioxidant in this embodiment are as follows:

[0041] The specific concentrations of the raw materials in the electrolytic aid in the electrolyte are as follows: graphene oxide: 5 mg / L, gelatin: 14 mg / L, cerium sulfate: 40 mg / L, sodium chloride: 20 mg / L, cellulose hydroxypropyl methyl ether: 6 mg / L, tetrahydrothiazolidinethione: 12 mg / L, polyethylene glycol: 8 mg / L, sodium phenyl polydisulfide propane sulfonate: 30 mg / L, polyethyleneimine: 35 mg / L; wherein the molecular weight of polyethyleneimine is 3000, and the number average molecular weight of gelatin is 5000.

[0042] The preparation method of the protective liquid comprises the following steps: respectively mixing 2-mercaptobenzoxazole, an antioxidant, ethylene glycol, vinyl trimethoxysilane, triethanolamine and dodecyl ethoxy sulfobetaine with an ethanol aqueous solution with a concentration of 35% and then uniformly preparing the protective liquid; wherein the concentration of 2-mercaptobenzoxazole in the protective liquid is 0.6 g / L, the concentration of the antioxidant is 1.0 g / L, the concentration of ethylene glycol is 1.5 ml / L, the concentration of vinyl trimethoxysilane is 2.5 ml / L, the concentration of triethanolamine is 2.5 ml / L, and the concentration of dodecyl ethoxy sulfobetaine is 4 g / L.

[0043] The preparation method of the antioxidant comprises the following steps:

[0044] S1, put the compound into acetonitrile with a mass 6 times that of the compound, and add 2-butynoic acid ethyl ester and aluminum chloride with a molar amount of 1.0 times that of the compound in sequence, and introduce nitrogen after mixing and stirring evenly, and raise the temperature of the mixed solution to 70°C under the protection of nitrogen, and stir and react at this temperature for 12 hours; after the reaction is completed, the resultant components are naturally cooled to room temperature, and then the resultant components are filtered and washed with water and the acetonitrile therein is evaporated, and the resulting liquid product is stored and used for standby;

[0045] S2, putting the liquid product into a reaction device, and adding 0.6 times the mass of palmityl alcohol and 3 times the mass of xylene of the liquid product in sequence, mixing and stirring evenly, introducing nitrogen to drive out the air in the reaction device, stirring and heating to 100° C., and then adding 0.04 times the mass of palmityl alcohol dibutyltin oxide thereto, and keeping the temperature for reaction for 15 hours; after the reaction is completed, adjusting the pH of the reaction product to 8.0, and then filtering, washing and distilling under reduced pressure to obtain a liquid component is an antioxidant;

[0046] Example 3

[0047] The production process of an oxidation-resistant electrolytic copper foil provided in this embodiment is basically the same as that in Embodiment 1, except that the specific composition of the electrolytic auxiliary agent and the preparation method of the antioxidant used are not exactly the same. The specific composition of the electrolytic auxiliary agent and the preparation method of the antioxidant in this embodiment are as follows:

[0048] The specific concentrations of the raw materials in the electrolytic aid in the electrolyte are as follows: graphene oxide: 6 mg / L, gelatin: 15 mg / L, cerium sulfate: 45 mg / L, sodium chloride: 25 mg / L, cellulose hydroxypropyl methyl ether: 8 mg / L, ethylene thiourea: 15 mg / L, polyethylene glycol: 10 mg / L, sodium 3-mercapto-1-propane sulfonate: 40 mg / L, polyethylene imine: 40 mg / L; wherein the molecular weight of polyethylene imine is 3000, and the number average molecular weight of gelatin is 5000.

[0049] The preparation method of the protective liquid comprises the following steps: respectively mixing 2-mercaptobenzoxazole, an antioxidant, ethylene glycol, vinyl tri(2-methoxyethoxy)silane, triethanolamine and dodecylethoxy sulfobetaine with an ethanol aqueous solution with a concentration of 40% and then uniformly preparing the protective liquid; wherein the concentration of 2-mercaptobenzoxazole in the protective liquid is 0.8 g / L, the concentration of the antioxidant is 1.2 g / L, the concentration of ethylene glycol is 2.0 ml / L, the concentration of vinyl tri(2-methoxyethoxy)silane is 3.0 ml / L, the concentration of triethanolamine is 3 ml / L, and the concentration of dodecylethoxy sulfobetaine is 5 g / L.

[0050] The preparation method of the antioxidant comprises the following steps:

[0051] S1, put the compound into acetonitrile with a mass 8 times that of the compound, and add 2-butynoic acid ethyl ester with a molar amount of 1.2 times that of the compound and 0.4 times that of boron trifluoride in sequence, mix and stir evenly, then introduce nitrogen, and raise the temperature of the mixed solution to 75°C under the protection of nitrogen, and stir and react at this temperature for 15 hours; after the reaction is completed, naturally cool the resultant components to room temperature, then filter and wash the resultant components with water and evaporate the acetonitrile therein, and store the resulting liquid product for standby use;

[0052] S2, putting the liquid product into a reaction device, and adding 0.8 times the mass of palmityl alcohol and 4 times the mass of xylene of the liquid product in sequence, mixing and stirring evenly, introducing nitrogen to drive out the air in the reaction device, stirring and heating to 110° C., and then adding 0.05 times the mass of palmityl alcohol dibutyltin oxide thereto, and keeping the temperature for reaction for 20 hours; after the reaction is completed, adjusting the pH of the reaction product to 8.5, and then filtering, washing and distilling under reduced pressure to obtain a liquid component is an antioxidant;

[0053] Comparative Example 1: The main difference between this example and Example 1 is that an equal amount of 2-mercaptobenzoxazole is used in this example to replace the antioxidant.

[0054] Comparative Example 2: The main difference between this example and Example 1 is that an equal amount of antioxidant is used in this example to replace 2-mercaptobenzoxazole.

[0055] Performance Testing

[0056] The relevant properties of the oxidation-resistant electrolytic copper foils provided in Examples 1 to 3 and Comparative Examples 1 to 2 were tested respectively, and the obtained test data were recorded in the following table:

[0057]

[0058]

[0059] By comparing and analyzing the relevant data in the table, it can be seen that the electrolytic copper foil produced by the present invention not only has excellent mechanical properties, but also has excellent anti-oxidation properties, which prolongs its service life to a certain extent and effectively guarantees the quality of the electrolytic copper foil. This shows that the oxidation-resistant electrolytic copper foil provided by the present invention has a broader market prospect and is more suitable for promotion.

[0060] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0061] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A production process for oxidation-resistant electrolytic copper foil, characterized in that: The following steps are involved: Step 1: Put high-purity copper wire with a purity of ≥99.97% into a sulfuric acid solution and heat it to dissolve it to obtain a copper sulfate solution; then add an electrolytic additive to the obtained copper sulfate solution, mix it evenly, and then transport the obtained electrolyte to an electrolytic cell and perform electrolysis at a temperature of 50-60°C; the obtained electrolytic copper foil is stored and used for standby; wherein, the copper in the copper sulfate solution is 2+ The concentration is 90~95g / L, SO4 2- The concentration is 100-110 g / L; Step 2: The electrolytic copper foil prepared in step 1 is transferred into a pickling tank for cleaning to remove the oxide film on the surface. The electrolytic copper foil is washed with water and then placed into a protective liquid and immersed at a temperature of 50 to 60° C. for 5 to 10 minutes to form an oxidation-resistant protective layer on the surface of the electrolytic copper foil. Step 3: Take out the electrolytic copper foil treated in step 2 from the protective liquid and wash the protective liquid remaining on its surface with ethanol, then dry the electrolytic copper foil; after drying, cut, slit and package it, and finally obtain the finished oxidation-resistant electrolytic copper foil.

2. The production process of an oxidation-resistant electrolytic copper foil according to claim 1, characterized in that: The electrolysis aid comprises graphene oxide, gelatin, cerium sulfate, sodium chloride, cellulose hydroxypropyl methyl ether, a filler, polyethylene glycol, a brightener and polyethyleneimine.

3. The production process of an oxidation-resistant electrolytic copper foil according to claim 2, characterized in that: The concentrations of the raw materials in the electrolytic aid in the electrolyte are as follows: graphene oxide: 3-6 mg / L, gelatin: 12-15 mg / L, cerium sulfate: 35-45 mg / L, sodium chloride: 20-25 mg / L, cellulose hydroxypropyl methyl ether: 5-8 mg / L, filler: 10-15 mg / L, polyethylene glycol: 6-10 mg / L, brightener: 20-40 mg / L, polyethylene imine: 35-40 mg / L; wherein the molecular weight of polyethylene imine is 1000-3000, and the number average molecular weight of gelatin is 1000-5000.

4. The production process of an oxidation-resistant electrolytic copper foil according to claim 1, characterized in that: The current intensity during the electrolysis process is 20000-30000A, and the flow rate of the electrolyte is 45-50m 3 / h.

5. The production process of an oxidation-resistant electrolytic copper foil according to claim 3, characterized in that: The filler is selected from any one of sodium mercaptoimidazole propanesulfonate, tetrahydrothiazolidinethione and ethylenethiourea.

6. The production process of an oxidation-resistant electrolytic copper foil according to claim 3, characterized in that: The brightener is selected from any one of sodium polydisulfide propane sulfonate, sodium phenyl polydisulfide propane sulfonate, and sodium 3-mercapto-1-propane sulfonate.

7. The production process of an oxidation-resistant electrolytic copper foil according to claim 1, characterized in that: The preparation method of the protective liquid comprises the following steps: respectively mixing 2-mercaptobenzoxazole, an antioxidant, ethylene glycol, a silane coupling agent, triethanolamine and dodecylethoxysulfobetaine with an ethanol aqueous solution with a concentration of 30-40% and then uniformly preparing the protective liquid; wherein the concentration of 2-mercaptobenzoxazole in the protective liquid is 0.5-0.8 g / L, the concentration of the antioxidant is 0.8-1.2 g / L, the concentration of ethylene glycol is 1.5-2.0 ml / L, the concentration of the silane coupling agent is 1.5-3.0 ml / L, the concentration of triethanolamine is 2-3 ml / L, and the concentration of dodecylethoxysulfobetaine is 3-5 g / L.

8. The production process of an oxidation-resistant electrolytic copper foil according to claim 7, characterized in that: The silane coupling agent is selected from any one of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tri (2-methoxyethoxy) silane.

9. The production process of an oxidation-resistant electrolytic copper foil according to claim 7, characterized in that: The preparation method of the antioxidant comprises the following steps: S1, putting the compound into acetonitrile with a mass of 5 to 8 times that of the compound, and sequentially adding 2-butynoic acid ethyl ester with a molar amount of 0.8 to 1.2 times that of the compound and a reaction accelerator with a molar amount of 0.2 to 0.4 times that of the compound, stirring and mixing evenly, introducing nitrogen, and raising the temperature of the mixed solution to 60 to 75° C. under the protection of nitrogen, stirring and reacting at this temperature for 10 to 15 hours; after the reaction is completed, naturally cooling the resultant components to room temperature, and then filtering and washing the resultant components with water and evaporating to remove the acetonitrile therein, and storing the obtained liquid product for standby use; S2, putting the liquid product into a reaction device, and adding palm alcohol with a mass of 0.5 to 0.8 times that of the liquid product and xylene with a mass of 2 to 4 times that of the liquid product in sequence, stirring and introducing nitrogen to drive out the air in the reaction device, stirring and heating to 90 to 110° C., and then adding dibutyltin oxide with a mass of 0.03 to 0.05 times that of the palm alcohol, and keeping the temperature for reaction for 10 to 20 hours; after the reaction is completed, adjusting the pH of the reaction product to 7.8 to 8.5, and then filtering, washing and distilling under reduced pressure to obtain a liquid component is an antioxidant; The structure of the compound is as follows:

10. The production process of an oxidation-resistant electrolytic copper foil according to claim 9, characterized in that: The reaction accelerator is selected from any one of triethylamine, aluminum chloride and boron trifluoride.

Citation Information

Cited By

  • Preparation method and application of five-membered azacyclo-monothiopropane sulfonate

    CN119176779A