Cold roll hard chromium electroplating process
By optimizing the composition of the electroplating solution and the treatment process, the problem of poor adhesion in hard chrome plating on cold rolling rolls was solved, resulting in high-quality and stable hard chrome plating and improving production efficiency and product quality.
Patent Information
- Application Number
- CN202411287705.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-08
AI Technical Summary
The existing hard chrome plating process for cold rolling rolls suffers from poor coating adhesion and low stability, leading to frequent roll replacements during the rolling process, which affects production efficiency and product quality.
A specific concentration of electroplating solution (230-250 g/L chromium anhydride, 2.5-2.8 g/L sulfuric acid, temperature 58-60℃) is used, and the solution is kept pure by circulating filtration equipment and reverse electrolysis treatment, so that the coating thickness is controlled to be 5-8 μm.
It improves the adhesion and wear resistance of the hard chrome plating on cold rolling rolls, ensures the stability of electroplating quality, extends the service life of the rolls, and reduces production costs.
Smart Images

Figure CN118910685A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cold rolling roller electroplating, and in particular to a cold rolling roller hard chromium electroplating process. Background Art
[0002] Cold rolling rolls are usually made of solid chrome steel, which is rough-ground and fine-ground to a surface roughness of 0.8-1.0μm, and then electroplated with a 3-8μm thick hard chrome layer before being put on the machine for steel plate rolling. Electroplating hard chrome can extend the interval of roller regrinding by about one-fold, ensuring the rolling quality of the rolls, improving the production efficiency of the rolling mill, and effectively reducing the rolling cost.
[0003] Cold-rolled steel rollers have relatively low rolling temperatures and high rolling pressures, which place high demands on the wear resistance of the rollers and the adhesion of the hard chrome plating of the rollers. The performance of the hard chrome plating produced by ordinary hard chrome electroplating processes is not stable. Sometimes, after rolling for 30-50 kilometers, the surface of the rolled product does not meet the requirements due to peeling of the plating, and the chrome-plated rollers need to be replaced in advance. Summary of the invention
[0004] The technical problem to be solved by the present invention is: in view of the deficiencies in the prior art, a hard chromium electroplating process for a cold rolling roller is provided, and the electroplating quality of the cold rolling roller is good and the stability is high.
[0005] In order to solve the above technical problems, the technical solution of the present invention is:
[0006] A cold rolling roller hard chrome electroplating process, wherein the electroplating process utilizes the electroplating solution in the plating tank to electroplate a hard chrome coating on the surface of the working part of the rolling roller, wherein the concentration of chromic anhydride in the electroplating solution is 230-250 g / l, the concentration of sulfuric acid is 2.5-2.8 g / l, and the concentration ratio of chromic anhydride to sulfuric acid in the electroplating solution is 100:1.1;
[0007] The temperature is controlled at 58-60℃ during the electroplating process.
[0008] Preferably, before each workpiece is placed in the plating tank, the specific gravity of the plating solution is measured using a Baume meter. If the measured value is between 21.5 and 23 O Be range, no adjustment is required;
[0009] If the measured value is less than 21.5 O Be, add chromic anhydride to the plating solution, if the measured value is greater than 23 O Be, add pure water to the plating solution.
[0010] Preferably, a circulating filter device is provided outside the plating tank, and after the chromic anhydride or pure water is added, the circulating filter device is turned on to circulate the electroplating solution for 3-8 minutes.
[0011] Preferably, the circulating filtration device comprises a filter, a circulating pump, a liquid outlet pipe and a liquid return pipe which are connected to each other, the inlet of the liquid outlet pipe is arranged in the plating tank, and the outlet of the liquid return pipe is arranged in the plating tank;
[0012] The circulating filter device starts circulating the electroplating solution at a preset interval to balance the temperature and specific gravity of the electroplating solution in the plating tank.
[0013] Preferably, at least one temperature sensor is provided in the plating tank, and when the temperature difference detected by any two of the temperature sensors is greater than a preset difference, the circulating filtering device is started to circulate the plating solution.
[0014] Preferably, a plurality of the temperature sensors are electrically connected to a temperature controller, and titanium tubes are arranged around the inner wall of the plating tank.
[0015] Preferably, after the plating tank under the workpiece is preheated, reverse electrolysis must be performed before normal electroplating, and the reverse electrolysis time is controlled to be 10-20s, the voltage is 5-8V, and the current is 1 / 3-1 / 2 of the normal electroplating current value.
[0016] Preferably, the plating solution is treated with a plating solution processor within a fixed period to remove metal impurities introduced into the plating solution due to reverse electrolysis before plating, thereby maintaining the purity of the plating solution.
[0017] Preferably, the hard chrome plating layer has a thickness of 5-8 μm.
[0018] Preferably, the sulfuric acid concentration in the plating solution is tested within a fixed period, and adjustments are made based on the test results to control the sulfuric acid concentration within the range of 2.5-2.8 g / l.
[0019] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0020] 1. This electroplating process fundamentally solves the rework caused by poor coating adhesion and high hardness due to large changes in plating solution process parameters and poor pre-plating treatment during the normal electroplating process. For example, if the concentration of the electroplating solution is as high as 230g / l chromic anhydride and 3.0g / l sulfuric acid, the plated coating will have high hardness and great brittleness, and will easily crack during use, resulting in defective products.
[0021] 2. Perform reverse electrolysis on the workpiece before electroplating in the plating tank to remove residual oil on the surface of the workpiece and form micro-etching on the surface of the workpiece to increase the adhesion of the coating.
[0022] 3. Since the workpiece is reversely electrolyzed in the plating tank, metal impurities harmful to the electroplating solution are generated. The present invention uses a plating solution processor to process the impurities in the electroplating solution, thereby maintaining the purity of the spot plating solution and keeping the quality of the hard chrome coating electroplated by the cold rolling roller stable.
[0023] 4. The hard chromium coating electroplated on the cold rolling roller of the present invention has very stable bonding strength and wear resistance, and can meet the use requirements of the steel rolling mill. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a microphotograph of the crystal phase of the hard chrome coating in Example 1;
[0025] Figure 2 is a microphotograph of the crystal phase of the hard chrome coating in Example 2;
[0026] Figure 3 is a microphotograph of the crystal phase of the hard chrome coating in Example 3;
[0027] Figure 4 This is a microscopic photograph of the crystal phase of the hard chrome coating in Example 4. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0029] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0030] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0031] A cold rolling roller hard chrome electroplating process, the electroplating process uses the electroplating solution in the plating tank to electroplate a hard chrome coating on the surface of the working part of the roller, the chromic anhydride concentration in the electroplating solution is 230-250g / l, the sulfuric acid concentration is 2.5-2.8g / l, and the concentration ratio of chromic anhydride to sulfuric acid in the electroplating solution is 100:1.1; the chromic anhydride is used as the main salt of the hard chrome electroplating solution to provide the required metal chromium ions for the coating, and the sulfuric acid is used as the hard chrome electroplating catalyst to help the metal chromium ions to precipitate smoothly in the electric field, playing a catalytic acceleration role.
[0032] The temperature is controlled at 58-60℃ during the electroplating process.
[0033] Before each workpiece is put into the plating tank, the specific gravity of the plating solution is measured using a Baume meter. If the measured value is between 21.5 and 23 O Be range, no adjustment is required;
[0034] If the measured value is less than 21.5 O Be, add chromic anhydride to the plating solution, if the measured value is greater than 23 O Be, add pure water to the electroplating solution. Since sulfuric acid is not consumed by electrolysis in the plating solution, when the chromic anhydride concentration changes in a wide range, the ratio of chromic anhydride concentration to sulfuric acid concentration will change greatly, resulting in unstable roller electroplating quality.
[0035] A circulating filter device is provided outside the plating tank. After the chromic anhydride or pure water is added, the circulating filter device is turned on to circulate the electroplating solution for 3-8 minutes.
[0036] The circulating filtration equipment comprises a filter, a circulating pump, a liquid outlet pipe and a liquid return pipe which are connected to each other, the inlet of the liquid outlet pipe is arranged in the plating tank, and the outlet of the liquid return pipe is arranged in the plating tank;
[0037] The circulating filter device starts circulating the electroplating solution at a preset interval to balance the temperature and specific gravity of the electroplating solution in the plating tank.
[0038] At least one temperature sensor is arranged in the plating tank. When the temperature difference detected by any two of the temperature sensors is greater than a preset difference, the circulating filtering device is started to circulate the plating solution.
[0039] Several of the temperature sensors are electrically connected to a temperature controller. Titanium tubes are arranged around the inner wall of the plating tank, and high-temperature steam or cooling water is passed through the temperature controller to heat or cool the plating solution to control the temperature of the plating solution at 58-60°C.
[0040] After the plating tank under the workpiece is preheated, reverse electrolysis must be carried out before normal electroplating. The reverse electrolysis time is controlled to be 10-20s, the voltage is 5-8V, and the current is 1 / 3-1 / 2 of the normal electroplating current value.
[0041] The plating solution is treated by a plating solution processor within a fixed period to remove metal impurities introduced into the plating solution by reverse electrolysis before plating, so as to keep the plating solution pure.
[0042] The thickness of the hard chrome plating layer is 5-8 μm.
[0043] Sulfuric acid is not consumed in the electroplating process, only loss occurs. Therefore, under normal circumstances, the concentration of sulfuric acid will not change much. Therefore, in actual work, the concentration of sulfuric acid in the plating solution is tested every week, and adjustments are made based on the test results to control the concentration of sulfuric acid within the range of 2.5-2.8g / l.
[0044] This electroplating process fundamentally solves the rework caused by poor coating adhesion and high hardness due to large changes in plating solution process parameters and poor pre-plating treatment during the normal electroplating process. For example, if the plating solution concentration is as high as 230g / l chromic anhydride and 3.0g / l sulfuric acid, the plated coating will have high hardness and great brittleness, and will easily crack during use, resulting in defective products.
[0045] Since the workpiece is reversely electrolyzed in the plating tank, metal impurities harmful to the plating solution are generated. The present invention uses a plating solution processor to process the impurities in the plating solution, thereby maintaining the purity of the plating solution and ensuring that the quality of the hard chrome plating layer electroplated on the cold rolling roller remains stable.
[0046] In order to more clearly illustrate the present invention, several embodiments are given below:
[0047] Example 1
[0048]
[0049] Example 2
[0050]
[0051]
[0052] Example 3
[0053]
[0054] Example 4
[0055]
[0056]
[0057] It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.
Claims
1. A cold rolling roller hard chrome electroplating process, wherein the electroplating process utilizes the electroplating solution in the plating tank to electroplate a hard chrome coating on the working part of the roller, and the process is characterized in that: The concentration of chromic anhydride in the electroplating solution is 230-250 g / l, the concentration of sulfuric acid is 2.5-2.8 g / l, and the concentration ratio of chromic anhydride to sulfuric acid in the electroplating solution is 100:1.1; The temperature is controlled at 58-60℃ during the electroplating process.
2. A cold rolling roller hard chrome electroplating process as claimed in claim 1, characterized in that: Before each workpiece is put into the plating tank, the specific gravity of the plating solution is measured using a Baume meter. If the measured value is between 21.5 and 23 O Be range, no adjustment is required; If the measured value is less than 21.5 O Be, add chromic anhydride to the plating solution, if the measured value is greater than 23 O Be, add pure water to the plating solution.
3. A cold rolling roller hard chrome electroplating process as claimed in claim 2, characterized in that: A circulating filter device is provided outside the plating tank. After the chromic anhydride or pure water is added, the circulating filter device is turned on to circulate the electroplating solution for 3-8 minutes.
4. A cold rolling roller hard chrome electroplating process as claimed in claim 3, characterized in that: The circulating filtration equipment comprises a filter, a circulating pump, a liquid outlet pipe and a liquid return pipe which are connected to each other, the inlet of the liquid outlet pipe is arranged in the plating tank, and the outlet of the liquid return pipe is arranged in the plating tank; The circulating filter device starts circulating the electroplating solution at a preset interval to balance the temperature and specific gravity of the electroplating solution in the plating tank.
5. A cold rolling roller hard chrome electroplating process as claimed in claim 4, characterized in that: At least one temperature sensor is arranged in the plating tank. When the temperature difference detected by any two of the temperature sensors is greater than a preset difference, the circulating filtering device is started to circulate the plating solution.
6. A cold rolling roller hard chrome electroplating process as claimed in claim 5, characterized in that: A plurality of the temperature sensors are electrically connected to a temperature controller, and titanium tubes are arranged around the inner wall of the plating tank.
7. A cold rolling roller hard chrome electroplating process as claimed in claim 1, characterized in that: After the plating tank under the workpiece is preheated, reverse electrolysis must be carried out before normal electroplating. The reverse electrolysis time is controlled to be 10-20s, the voltage is 5-8V, and the current is 1 / 3-1 / 2 of the normal electroplating current value.
8. A cold rolling roller hard chrome electroplating process as claimed in claim 7, characterized in that: The plating solution is treated by a plating solution processor within a fixed period to remove metal impurities introduced into the plating solution by reverse electrolysis before plating, so as to keep the plating solution pure.
9. A cold rolling roller hard chrome electroplating process as claimed in claim 1, characterized in that: The thickness of the hard chrome plating layer is 5-8 μm.
10. A cold rolling roller hard chrome electroplating process as claimed in claim 1, characterized in that: In a fixed period, the sulfuric acid concentration in the plating solution is tested and adjusted according to the test results to control the sulfuric acid concentration within the range of 2.5-2.8g / l.