Filament capable of absorbing electromagnetic waves and preparation method thereof

The preparation of absorbed electromagnetic wavelength filaments through magnetic stretch spinning system solves the problems of low treatment efficiency and environmental pollution of marine plastic waste, improves fiber performance and environmental protection, and realizes the protection of the marine environment and the recycling of resources.

CN118910744AActive Publication Date: 2024-11-08JIANGSU YONGYIN CHEM FIBER
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410876031.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-08
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The prior art has problems of low treatment efficiency, high cost and environmental pollution when dealing with marine plastic waste, and the problems of agglomeration and heat waste are prone to occur in traditional fiber preparation processes.

Method used

Using magnetic stretch spinning system, the absorbed electromagnetic wavelength filaments are prepared by using raw materials such as marine plastics and nano-inorganic magnetic materials to achieve precise stretching and recycling through twin-screw extruders, magnetic heating devices and multi-stage magnetic stretching devices. Reduce energy consumption.

Benefits of technology

It improves the tensile mechanical strength and electromagnetic shielding performance of the fiber, reduces process complexity and labor costs, protects the marine environment, and realizes the recycling of resources and emission reduction of carbon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910744A_ABST
    Figure CN118910744A_ABST
Patent Text Reader

Abstract

The invention relates to an electromagnetic wave absorbing filament and a preparation method thereof, and belongs to the technical field of functional fibers. According to the preparation method, a magnetic stretching spinning system is used as a generating device, a double-screw extruder, a magnetic heating device and a multi-stage magnetic stretching device are included, and the preparation method comprises the following steps that S1, marine plastic, a nano inorganic magnetic material, a nano modifier, filler, an auxiliary and a silane coupling agent are added into the double-screw extruder to be evenly mixed, and a mixed material is obtained; the functional master batch is obtained through granulation; the marine plastic is selected from PP plastic and / or PET plastic; s2, magnetically heating the functional master batch through a magnetic heating device to obtain a molten master batch; s3, the molten master batch passes through a pinhole plate, and nascent fibers are obtained; s4, stretching the nascent fibers through a multi-stage magnetic stretching device to obtain the electromagnetic wave absorbing filaments which are uniform in distribution, excellent in electromagnetic shielding capability and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional fibers, and in particular relates to a fiber that absorbs electromagnetic wavelengths and a preparation method thereof. Background Art

[0002] At present, marine debris has become one of the major global environmental problems. Plastic is the main type of marine debris. There are three ways to deal with plastic waste. The first way is to transport it directly to the incineration plant for incineration, but incineration produces a large amount of toxic and harmful gases, which pollutes the environment; plastic waste cannot be recycled, which is not conducive to emission reduction and carbon reduction. The second way is that during the collection of marine plastics, first, the plastic is flattened by manual or compression tools to reduce the volume of the plastic; then, it is packed and transported to the plastic disposal plant for treatment; then, the received plastics are disassembled, sorted, and cleaned in the factory. The disassembly mainly separates the bottle cap and the bottle body. The bottle cap is usually made of PP material, and the bottle body is usually made of PET material. Then, it is sorted according to the material, and the sorted plastic waste is cleaned; finally, the cleaned plastic waste is recycled and reused. Disassembly, sorting, and cleaning are all manual operations, occupying a large amount of factory area to stack plastic waste. The overall process is complicated, the processing time is long, and the recycling efficiency is low. The third method is to use a plastic crusher to crush the collected, disassembled, sorted and cleaned plastic waste. The existing plastic crusher only has the crushing function, without automatic feeding, automatic cleaning, impurity removal and other functions. It is then sorted according to the material, and the sorted plastic waste is cleaned; finally, the cleaned plastic waste is recycled and reused. Disassembly, sorting and cleaning are all manual operations, which occupy a large amount of factory area to stack plastic waste. The overall process is complicated, the processing time is long, and the recycling efficiency is low. If marine materials can be directly used without cleaning, a lot of time can be saved.

[0003] Chinese invention patent CN115012055A discloses a method for preparing a flexible stretchable magnetic wire and a flexible stretchable magnetic wire. A hollow spiral structure mold is used to mix magnetic particles and an organic polymer to form a colloidal mixture; the colloidal mixture is stirred until it becomes viscous and poured into a mold; the colloidal mixture is allowed to stand, solidified, and a flexible magnetic wire is obtained after post-treatment. The basic principle is to use liquid spinning technology to extrude a mixture of organic polymers and magnetic particles and then pour it into a corresponding mold. However, agglomeration is prone to occur during the solidification process. Without stretching treatment, the tensile strength and elastic modulus of the prepared fiber are reduced.

[0004] Chinese invention patent CN109859901A discloses a stretching device for producing ultra-fine electromagnetic wires, including a base, a first rotating shaft, a second rotating shaft and a third rotating shaft. The wire rollers are driven to rotate by setting three sets of rotating shafts, and the three sets of rotating shafts are set to different rotation speeds. The electromagnetic wires are stretched twice during the rotation of the wire rollers, and the drawing efficiency of the ultra-fine electromagnetic wires is improved; the surface of the electromagnetic wires is polished by setting a polishing device to ensure the uniformity and quality of the electromagnetic wires, and for different wire diameters, the length of the electric push rod and the pressure of the spring itself can be adjusted to perform polishing. The wire is stretched by a local point force method, which is prone to produce weak nodes during stretching, affecting the quality of the yarn.

[0005] Chinese invention patent CN114427136A discloses a fiber heat stretching and shaping device and a stretching method thereof, comprising: a heater; an oil tank, which is placed on the heater and has a refueling port on the top, and the center of the top surface of the oil tank is concave downward to form a heating tank. The fiber is evenly contacted with the heating tank until the fiber softens by heating in an oil bath, and resources are wasted during the heating process. The oil agent needs to be removed after heat stretching, which is cumbersome and increases costs. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides an electromagnetic wavelength absorbing yarn and a preparation method thereof, which uses a magnetic stretching spinning system as a generating device, effectively utilizes substances in seawater, and can also reduce energy consumption during stretching. Precise stretching is not only beneficial to purifying the marine environment, but also can be recycled to reduce emissions and carbon emissions.

[0007] The first object of the present invention is to provide a method for preparing electromagnetic wavelength absorbing yarn, which uses a magnetic stretching spinning system as a generating device, including a twin-screw extruder, a magnetic heating device and a multi-stage magnetic stretching device, a pinhole plate is arranged between the magnetic heating device and the multi-stage magnetic stretching device; the magnetic heating device includes NS permanent magnets and a spiral spinning pipeline arranged between the NS permanent magnets, and a plurality of cutting magnetic flux lines are arranged in the spiral spinning pipeline; the inlet end and the outlet end of the spiral spinning pipeline are respectively connected to the outlet of the twin-screw extruder and the pinhole plate; the preparation method comprises the following steps,

[0008] S1, adding marine plastic, nano inorganic magnetic material, nano modifier, filler, additive and silane coupling agent into a twin-screw extruder and mixing them evenly, and obtaining functional masterbatch by granulation; the marine plastic is selected from PP plastic and / or PET plastic;

[0009] S2, the functional masterbatch is magnetically heated by a magnetic heating device to obtain a molten masterbatch;

[0010] S3, the molten masterbatch passes through a pinhole plate to obtain primary fibers;

[0011] S4. The nascent fiber is stretched by a multi-stage magnetic stretching device to obtain the electromagnetic wavelength absorbing fiber.

[0012] In one embodiment of the present invention, the spiral radius of the spiral spinning pipe gradually increases, so that the diameter of the spiral spinning pipe remains unchanged, ensuring that the flow rate generates a smooth transition curve based on the original spiral line, avoiding pipe blockage. The flow field is smooth and the contact area is increased at the same time; the initial spiral radius is 10cm-20cm, the number of turns is 10-20; the diameter of the spiral spinning pipe is 2cm-4cm; the angle between the plane where the end face of the spiral spinning pipe is located and the horizontal plane is 5°-20°; the angle formed by the projection of the central axis of the spiral spinning pipe on the plane where the NS permanent magnet is located is 10°-30°.

[0013] In one embodiment of the present invention, the number of the cutting magnetic fluxion line elements is 500-1500; the connection mode of the cutting magnetic fluxion line elements is selected from series connection and / or parallel connection. The cutting magnetic fluxion line elements perform cutting magnetic fluxion line movement, and the cutting magnetic fluxion line elements are made of metal conductor material to form a closed loop.

[0014] In one embodiment of the present invention, the pinhole plate is provided with 36-72 groups of pinholes, and the stretching diameter of the pinholes is 0.2cm-1cm.

[0015] In one embodiment of the present invention, in S1, the nano inorganic magnetic material is selected from one or more of neodymium iron boron magnetic material, neodymium nickel cobalt magnetic material, ferroferric oxide magnetic material, chromium dioxide magnetic material, and cobalt-iron oxide magnetic material;

[0016] and / or, the nano-modifier is selected from titanium dioxide and / or silicon dioxide;

[0017] And / or, the filler is selected from one or more of carbon nanofibers, carbon nanotubes and carbon fibers;

[0018] And / or, the auxiliary agent is selected from one or more of citric acid, sodium citrate, potassium citrate, oxalic acid, sodium oxalate or potassium oxalate;

[0019] And / or, the silane coupling agent is selected from one or more of KH550, KH560 and KH570.

[0020] In one embodiment of the present invention, in S1, the mass ratio of the marine plastic, nano inorganic magnetic material, nano modifier, filler, additive and silane coupling agent is (60-80): (20-40): (1-10): (1-10): (1.5-9): (0.5-1). Marine plastic is taken from marine garbage, a renewable raw material, and is an environmentally friendly material. Nano inorganic magnetic material brings electromagnetic shielding effect to the material. Nano modifier improves the electromagnetic shielding effect and further improves the filament forming performance, improves the toughness and strength of the filament during use, marine plastic, inorganic magnetic material, nano modifier, a large number of copolymers with active functional groups, and the silane coupling agent added later further enhances the adhesion, improves the bonding strength, and prolongs the service life.

[0021] In one embodiment of the present invention, in S1, during the granulation process, the twin-screw extruder is divided into five heating zones, the heating temperature of zone one is 260°C, the heating temperature of zone two is 275°C, the heating temperature of zone three is 280°C, the heating temperature of zone four is 278°C, and the heating temperature of zone five is 265°C.

[0022] In one embodiment of the present invention, in S2, during the magnetic heating process, the advancement speed of the functional masterbatch is 0.1m / s-2m / s, and the magnetic induction intensity is 600mT-1000mT. By controlling the constant tension of the primary fiber during stretching, the fiber is stretched by magnetic force, and the entire fiber is stressed, rather than the stress concentrated at one point in the traditional way. Different stretching sections are used to adapt to the use of fibers in different states. The coil tube determines the size of the magnetic field, and different turns provide different stresses.

[0023] In one embodiment of the present invention, in S4, the number of stages of the multi-stage magnetic stretching device is 2-6, the elongation ratio is 1:(30-50), and the number of turns of a single-stage solenoid is 1-100.

[0024] In one embodiment of the present invention, in S4, the stretching process parameters are: temperature of 90°C-130°C, output power of 500W-1000W, and output current of 2A-8A.

[0025] The second object of the present invention is to provide a wire that absorbs electromagnetic wavelengths and is prepared by the method described above.

[0026] The technical solution of the present invention has the following advantages over the prior art:

[0027] (1) The multi-stage magnetic stretching device used in the preparation method of the present invention forms a uniform magnetic field after being energized during hot stretching, and then forms magnetic field lines that are evenly distributed downward, converting the point force in traditional stretching into the force of the entire filament, reducing weak nodes, and improving the tensile mechanical strength. The single filaments are evenly dry, which can greatly reduce the unevenness. The magnetic heating device is used to perform magnetically generated electric heating from the inside to the outside, which makes the heating part more precise and further reduces heat loss.

[0028] (2) The preparation method of the present invention uses marine plastic as the base material, solves marine garbage, protects the marine environment, and reduces the pollution to the environment caused by the production of polymer materials; and the marine plastic does not need to be washed in large quantities before use, which reduces costs. Seawater immersion causes the marine plastic to carry many marine substances. While solving environmental problems, it utilizes marine resources, eliminates the washing step in the traditional method, and reduces labor costs. Using existing materials not only saves resources but also protects the environment.

[0029] (3) The preparation method described in the present invention uses marine plastic as raw material. The marine plastic is immersed in seawater and adheres to conductive particles such as sodium chloride and magnesium chloride in the ocean. It can conduct electricity in a molten state. A large amount of copolymers with active functional groups and a silane coupling agent added later further enhance the adhesion. The silane coupling agent is used to improve the compatibility of each raw material component, so as to give full play to the mutual coordination and synergy of each raw material component. The excellent performance of each raw material component is comprehensively utilized, and the self-assembly of nano-inorganic magnetic materials during hot stretching and the loose and porous stacking morphology caused by the filler can synergistically improve its electromagnetic shielding ability and effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0031] Figure 1 is a schematic diagram of the magnetic stretch spinning system of the present invention;

[0032] Figure 2 A cross-sectional view of a spiral spinning pipeline of a magnetic heating device of the present invention;

[0033] Figure 3 Schematic diagram of the angle between the plane where the end surface of the spiral spinning pipe of the present invention is located and the horizontal plane;

[0034] Figure 4 It is a schematic diagram of the angle formed by the projection of the central axis of the spiral spinning pipeline of the present invention on the plane where the NS permanent magnet is located;

[0035] Figure 5 It is a multi-level top view of the pinhole plate of the present invention;

[0036] Figure 6 It is a schematic diagram of the multi-stage magnetic stretching device of the present invention;

[0037] Explanation of the reference numerals: 1-twin-screw extruder, 2-magnetic heating device, 21-spiral spinning pipe, 211-cutting magnetic flux element, 3-pinhole plate, 31-pinhole, 32-stretching tube diameter, 33-air flow hole, 4-multi-stage magnetic stretching device, 41 is a primary magnetic stretching device, and 42 is a secondary magnetic stretching device. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0040] The electromagnetic wavelength absorbing yarn of the present invention is produced by a magnetic stretching spinning system, and its structure is as follows Figure 1-6 As shown, it includes a twin-screw extruder 1, a magnetic heating device 2 and a multi-stage magnetic stretching device 4, a pinhole plate 3 is arranged between the magnetic heating device and the multi-stage magnetic stretching device; the magnetic heating device includes NS permanent magnets and a spiral spinning pipe 21 arranged between the NS permanent magnets, and a plurality of cutting magnetic induction line elements 211 are arranged in the spiral spinning pipe 21; the inlet end and the outlet end of the spiral spinning pipe 21 are respectively connected to the outlet of the twin-screw extruder 1 and the pinhole plate 3; the pinhole plate 3 is provided with an air flow hole 33; marine plastics, nano inorganic magnetic materials, nano modifiers, fillers, additives and silane coupling agents are added The functional masterbatch is introduced into the twin-screw extruder 1 for mixing and granulation to obtain the functional masterbatch; the functional masterbatch enters the spiral spinning pipe 21 in the magnetic heating device 2, and the cutting magnetic flux line element 211 in the spiral spinning pipe 2 is used to cut the magnetic flux line to generate current to magnetically heat the functional masterbatch to obtain the molten masterbatch; the molten masterbatch passes through the pinhole 31 in the pinhole plate 3 under the spiral spinning pipe 2, and forms the primary fiber through the stretching tube 32; the primary fiber is stretched by the multi-stage magnetic stretching device 4 (the primary magnetic stretching device 41 and the secondary magnetic stretching device 42, etc.) to obtain the electromagnetic wavelength absorbing fiber.

[0041] Example 1

[0042] The electromagnetic wavelength absorbing wire and the preparation method thereof of the present invention specifically include the following steps:

[0043] S1. Add marine plastic, nano-NdFeB magnetic material, nano-modifier titanium dioxide, filler carbon nanofiber, additive citric acid and silane coupling agent KH550 in a mass ratio of 65:25:5:5:5:0.5 into a twin-screw extruder 1 for mixing, and granulate to obtain a functional masterbatch; wherein, during the granulation process, the twin-screw extruder is divided into five heating zones, the heating temperature of zone 1 is 260°C, the heating temperature of zone 2 is 275°C, the heating temperature of zone 3 is 280°C, the heating temperature of zone 4 is 278°C, and the heating temperature of zone 5 is 265°C;

[0044] S2, the functional masterbatch enters the spiral spinning pipe 21 in the magnetic heating device 2 at a speed of 1m / s, and the cutting magnetic flux line element 211 in the spiral spinning pipe 2 is used to cut the magnetic flux line movement to generate current to magnetically heat the functional masterbatch to obtain the molten masterbatch; wherein, the spiral radius of the spiral spinning pipe 21 gradually increases, the initial spiral radius is 20cm, and the number of turns is 20; the diameter of the spiral spinning pipe is 4cm; the angle α between the plane where the end face of the spiral spinning pipe is located and the horizontal plane is 20°; the angle β formed by the projection of the central axis of the spiral spinning pipe on the plane where the NS permanent magnet is located is 30°; the number of the cutting magnetic flux line elements 211 is 500, which are connected in series, and the magnetic induction intensity is 1000mT;

[0045] S3, the molten masterbatch passes through 36 groups of pinholes 31 with a drawing tube diameter 32 of 0.2 cm in the pinhole plate 3 below the spiral spinning pipe 2 to form primary fibers;

[0046] S4. The nascent fiber is stretched by a multi-stage magnetic stretching device 4 to obtain a filament that absorbs electromagnetic wavelengths; wherein the number of stages of the multi-stage magnetic stretching device is 4, the elongation ratio is 1:30, and the number of turns of the single-stage solenoid is 2, 10, 20, and 60 respectively; the stretching process parameters are: temperature is 100°C, output power is 880W, and output current is 4A.

[0047] Example 2

[0048] The electromagnetic wavelength absorbing wire and the preparation method thereof of the present invention specifically include the following steps:

[0049] S1. Add marine plastic, nano-NdFeB magnetic material, nano-modifier titanium dioxide, filler carbon nanofiber, additive citric acid and silane coupling agent KH550 into a twin-screw extruder 1 at a mass ratio of 60:23:2:8:6:1 for mixing, and granulate to obtain functional masterbatch; wherein, during the granulation process, the twin-screw extruder is divided into five heating zones, the heating temperature of zone 1 is 260°C, the heating temperature of zone 2 is 275°C, the heating temperature of zone 3 is 280°C, the heating temperature of zone 4 is 278°C, and the heating temperature of zone 5 is 265°C;

[0050] S2, the functional masterbatch enters the spiral spinning pipe 21 in the magnetic heating device 2 at a speed of 1.5m / s, and the cutting magnetic flux line element 211 in the spiral spinning pipe 2 is used to cut the magnetic flux line movement to generate current to magnetically heat the functional masterbatch to obtain the molten masterbatch; wherein, the spiral radius of the spiral spinning pipe 21 gradually increases, the initial spiral radius is 15cm, and the number of turns is 15; the diameter of the spiral spinning pipe is 3cm; the angle α between the plane where the end face of the spiral spinning pipe is located and the horizontal plane is 15°; the angle β formed by the projection of the central axis of the spiral spinning pipe on the plane where the NS permanent magnet is located is 25°; the number of the cutting magnetic flux line elements 211 is 1000, which are connected in series, and the magnetic induction intensity is 800mT;

[0051] S3, the molten masterbatch passes through 36 groups of pinholes 31 with a drawing tube diameter 32 of 0.2 cm in the pinhole plate 3 below the spiral spinning pipe 2 to form primary fibers;

[0052] S4. The nascent fiber is stretched by a multi-stage magnetic stretching device 4 to obtain a filament that absorbs electromagnetic wavelengths; wherein the multi-stage magnetic stretching device has 6 stages, an elongation ratio of 1:50, and the number of turns of the single-stage solenoid is 2, 5, 10, 20, 40, and 100, respectively; the stretching process parameters are: a temperature of 130°C, an output power of 660W, and an output current of 3A.

[0053] Example 3

[0054] The electromagnetic wavelength absorbing wire and the preparation method thereof of the present invention specifically include the following steps:

[0055] S1. Add marine plastic, nano-ferroferric oxide magnetic material, nano-modifier silica, filler carbon nanotubes, additive sodium citrate and silane coupling agent KH550 in a mass ratio of 65:25:5:5:5:0.5 into a twin-screw extruder 1 for mixing, and granulate to obtain a functional masterbatch; wherein, during the granulation process, the twin-screw extruder is divided into five heating zones, the heating temperature of zone 1 is 260°C, the heating temperature of zone 2 is 275°C, the heating temperature of zone 3 is 280°C, the heating temperature of zone 4 is 278°C, and the heating temperature of zone 5 is 265°C;

[0056] S2, the functional masterbatch enters the spiral spinning pipe 21 in the magnetic heating device 2 at a speed of 2m / s, and the cutting magnetic flux line element 211 in the spiral spinning pipe 2 is used to cut the magnetic flux line movement to generate current to magnetically heat the functional masterbatch to obtain the molten masterbatch; wherein, the spiral radius of the spiral spinning pipe 21 gradually increases, the initial spiral radius is 10cm, and the number of turns is 10; the diameter of the spiral spinning pipe is 2cm; the angle α between the plane where the end face of the spiral spinning pipe is located and the horizontal plane is 20°; the angle β formed by the projection of the central axis of the spiral spinning pipe on the plane where the NS permanent magnet is located is 10°; the number of the cutting magnetic flux line elements 211 is 1500, which are connected in series, and the magnetic induction intensity is 600mT;

[0057] S3, the molten masterbatch passes through 36 groups of pinholes 31 with a drawing tube diameter 32 of 0.2 cm in the pinhole plate 3 below the spiral spinning pipe 2 to form primary fibers;

[0058] S4. The nascent fiber is stretched by a multi-stage magnetic stretching device 4 to obtain a filament that absorbs electromagnetic wavelengths; wherein the multi-stage magnetic stretching device has 4 stages, an elongation ratio of 1:45, and the number of turns of a single-stage solenoid is 2, 10, 30, and 90, respectively; the stretching process parameters are: a temperature of 120°C, an output power of 660W, and an output current of 3A.

[0059] Comparative Example 1

[0060] It is basically the same as Example 1, except that: compared with Example 1, the magnetic heating method is replaced by the traditional electric current heating method, and heating is performed from the outside to the inside. The masterbatch is a poor conductor of heat, and a larger power is required to melt the masterbatch. Different stretching rollers are used for stretching, and speed difference is used for stretching, resulting in broken ends and hairy fibers at the subsequent stretching stress points.

[0061] Comparative Example 2

[0062] The method is basically the same as Example 1, except that the marine plastic is replaced with a plastic bottle that has not been soaked in seawater, and no substances contained in seawater are added. Some conductive particles are not contained therein, and during the melting process, the resistance becomes larger, the current becomes smaller, the heat generated is reduced, and the filament is not completely melted, resulting in unevenness.

[0063] Comparative Example 3

[0064] The method is basically the same as Example 1, except that: nano-modifier silica and silane coupling agent are not added, the bonding performance of each component is reduced, breakage occurs during stretching, and the fiber strength is reduced.

[0065] Comparative Example 4

[0066] The method is basically the same as Example 1, except that: no nano-iron tetroxide magnetic material is added, and when the fiber is stretched in the magnetic field at the end, the stretching force is significantly reduced, the fiber orientation degree is reduced, and the thickness of the primary fiber changes little when passing through the stretching pipe.

[0067] Test Case

[0068] The electromagnetic shielding properties of the filaments prepared in Examples 1-3 and Comparative Examples 1-4 were tested:

[0069] (1) Electromagnetic shielding performance: The electromagnetic shielding performance test is carried out using a microwave network vector analyzer with a test frequency of GHz2-18GHz;

[0070] (2) Breaking strength: The breaking strength of the fiber is measured using a strength tester;

[0071] (3) Fiber diameter unevenness: According to the formula CV% = S / X*100%, where S is the standard deviation and x is the mean value;

[0072] (4) Orientation: The fiber orientation was calculated using the following formula: ) calculation; where θ represents the molecular chain parallel to the orientation direction, and f represents the orientation degree;

[0073] Table 1 shows the relevant properties of the unmodified polyester fiber and the modified polyester fiber finally measured:

[0074] Table 1

[0075] Sample Electromagnetic shielding (dB) Breaking strength(N) Fiber diameter unevenness (%) Orientation Example 1 30.1 5.8 0.94 0.92 Example 2 36.2 4.7 0.96 0.90 Example 3 28.7 5.5 0.85 0.91 Comparative Example 1 12.6 3.2 1.58 0.88 Comparative Example 2 9.8 2.7 4.78 0.86 Comparative Example 3 10.2 2.3 3.52 0.72 Comparative Example 4 0.5 1.9 2.35 0.69

[0076] As can be seen from Table 1, the fiber of the embodiment has better performance. It can be seen from the comparison of Example 1 and Comparative Example 1 that the magnetic heating and multi-stage magnetic stretching device used, the fiber has better orientation and breaking strength. After reducing the knots, the breaking strength of the fiber is significantly improved. The heating method from the inside to the outside is adopted, and the non-traditional pipe wall heating is used to reduce the heat loss in convection, improve the heating efficiency, accelerate the fusion of materials between the masterbatch, and the uniform dispersion of functional materials, and improve the electromagnetic shielding performance of the fiber as a whole. A large number of hydrogen bonds are formed from the inside, which further improves the orientation of the fiber, and the fiber unevenness rate decreases, thereby forming a fiber with better integrity. It can be seen from the comparison of Example 1 and Comparative Examples 2-4 that the added magnetic particles and marine plastics are interconnected, which greatly improves the electromagnetic shielding efficiency, and the addition of the modifier is to extend the use of the fiber, further increase the bonding effect, make it more closely connected, improve the mechanical strength, and expand the scope of use. The added modifier can thicken on the one hand and introduce new functional groups on the other hand.

[0077] The components of the embodiment effectively enhance the different functions of the fiber, and the components work together to enhance the efficiency. The functional groups contained in the components are utilized to form different chemical bonds, thereby strengthening the fusion between the components.

[0078] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing a wire that absorbs electromagnetic wavelengths, characterized in that: The magnetic stretching spinning system is used as a generating device, including a twin-screw extruder, a magnetic heating device and a multi-stage magnetic stretching device, a pinhole plate is arranged between the magnetic heating device and the multi-stage magnetic stretching device; the magnetic heating device includes NS permanent magnets and a spiral spinning pipeline arranged between the NS permanent magnets, and a plurality of cutting magnetic flux lines are arranged in the spiral spinning pipeline; the inlet end and the outlet end of the spiral spinning pipeline are respectively connected to the outlet of the twin-screw extruder and the pinhole plate; the preparation method comprises the following steps, S1. Add marine plastic, nano inorganic magnetic material, nano modifier, filler, additive and silane coupling agent into a twin-screw extruder and mix them evenly, and obtain functional masterbatch by granulation; the marine plastic is selected from PP plastic and / or PET plastic; S2, the functional masterbatch is magnetically heated by a magnetic heating device to obtain a molten masterbatch; S3, the molten masterbatch passes through a pinhole plate to obtain primary fibers; S4. The nascent fiber is stretched by a multi-stage magnetic stretching device to obtain the electromagnetic wavelength absorbing fiber.

2. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: The spiral radius of the spiral spinning pipe gradually increases, the initial spiral radius is 10cm-20cm, and the number of turns is 10-20; the diameter of the spiral spinning pipe is 2cm-4cm; the angle between the plane where the end face of the spiral spinning pipe is located and the horizontal plane is 5°-20°; the angle formed by the projection of the central axis of the spiral spinning pipe on the plane where the NS permanent magnet is located is 10°-30°.

3. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: The number of the cutting magnetic flux lines elements is 500-1500; the connection mode of the cutting magnetic flux lines elements is selected from series connection and / or parallel connection.

4. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: The pinhole plate is provided with 36-72 groups of pinholes, and the stretching diameter of the pinholes is 0.2cm-1cm.

5. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: In S1, the nano inorganic magnetic material is selected from one or more of neodymium iron boron magnetic material, neodymium nickel cobalt magnetic material, ferroferric oxide magnetic material, chromium dioxide magnetic material, and cobalt-iron oxide magnetic material; and / or, the nano-modifier is selected from titanium dioxide and / or silicon dioxide; And / or, the filler is selected from one or more of carbon nanofibers, carbon nanotubes and carbon fibers; And / or, the auxiliary agent is selected from one or more of citric acid, sodium citrate, potassium citrate, oxalic acid, sodium oxalate or potassium oxalate; And / or, the silane coupling agent is selected from one or more of KH550, KH560 and KH570.

6. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: In S1, the mass ratio of the marine plastic, nano-inorganic magnetic material, nano-modifier, filler, additive and silane coupling agent is (60-80):(20-40):(1-10):(1-10):(1.5-9):(0.5-1).

7. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: In S2, during the magnetic heating process, the advancement speed of the functional masterbatch is 0.1m / s-2m / s, and the magnetic induction intensity is 600mT-1000mT.

8. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: In S4, the number of stages of the multi-stage magnetic stretching device is 2-6, the elongation ratio is 1:(30-50), and the number of turns of a single-stage solenoid is 1-100.

9. The method for preparing electromagnetic wavelength absorbing wire according to claim 1, characterized in that: In S4, the stretching process parameters are: temperature of 90°C-130°C, output power of 500W-1000W, and output current of 2A-8A.

10. An electromagnetic wavelength absorbing filament prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Stretching device for producing ultra-fine electromagnetic wire

    CN109859901A

  • Fiber hot stretching shaping device and stretching method thereof

    CN114427136A

  • Preparation method of flexible stretchable magnetic wire and flexible stretchable magnetic wire

    CN115012055A

  • Magnetized-and-demagnetized Lyocell fiber high-quality textile process

    CN110846776A

  • Preparation method of graphene antibacterial melt-blown cloth and application thereof

    CN111636147A