Spinning technology of high-elongation PEDOT: PSS / PEG conductive fiber

By adding PEG and DMSO to the spinning liquid and using Cu2+ and Li+ to assist molding, the problem of insufficient tensileability of PEDOT:PSS-based fibers in wet spinning technology is solved, which significantly improves the tensileability and electrical conductivity of the fibers , expanding its application in the field of wearable electronics.

CN118910766APending Publication Date: 2024-11-08NINGBO INST OF NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410942014.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The PEDOT:PSS-based fibers prepared by the existing wet spinning technology are insufficient in tensile properties, which limits their application in the field of wearable electronics.

Method used

By adding PEG solid particles and DMSO solvent to the spinning liquid, combining Cu2+ and Li+ assisted molding, a single-axis spinning technology and an environmentally friendly solidification bath are used to form a stable PEDOT:PSS/PEG cross-linking network to improve fiber stretching and conductivity.

Benefits of technology

It significantly improves the tensile and electrical conductivity of the fiber, making it an important functional material in the field of flexible electronic devices, and expands its application potential in the field of wearable electronics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a spinning technology of PEDOT: PSS / PEG conductive fibers, and relates to the technical field of preparation of organic conductive polymer-based composite fibers.PEG solid particles and a DMSO solvent are added into a PEDOT: PSS spinning solution, a blended spinning solution is vertically pumped into a mixed coagulating bath at a constant speed by an injection pump through a single-shaft spinning needle, the mixed coagulating bath is a mixed solution composed of ethyl alcohol, water, copper chloride and lithium chloride, and the mixed coagulating bath is subjected to spinning and spinning to obtain the PEDOT: PSS / PEG conductive fibers. Curing and forming the blended spinning solution through a mixed coagulating bath, entering an EG (Ethylene Glycol) bath, washing with water, collecting, heating the collected fiber in a vacuum drying oven at 50 DEG C for 3 hours, and finally preparing the high-tensile PEDOT: PSS / PEG conductive fiber. The fiber is prepared by adopting a wet spinning technology, the tensile property is improved by adding PEG solid particles and a DMSO solvent into a spinning solution, the tensile property and spinnability are improved by adding Cu < 2 + > and Li < + > into a coagulating bath to assist in forming, the conductivity is improved by EG post-treatment, and the fiber becomes a functional material with important development potential in the field of flexible electronic devices due to the excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of organic conductive polymer-based composite fibers, and in particular to a spinning technology for high-elongation PEDOT:PSS / PEG conductive fibers. Background Art

[0002] Poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS) is formed by the complexation of two polymers, PEDOT and PSS. The aqueous dispersion of PEDOT:PSS has strong environmental stability and has become a popular conductive polymer material. Wet spinning technology is the main method for preparing PEDOT:PSS-based fibers due to its low cost and controllable quality. Its advantage is that it can prepare continuously spinnable fibers. Among them, wet-spun PEDOT:PSS fiber-based materials have become functional materials with important development potential in the field of flexible electronic devices due to their excellent conductive properties and flexibility, and have been widely used in the field of flexible electronic devices. However, the PEDOT:PSS-based fibers prepared by wet spinning technology are not stretchable enough, which limits their application in the field of wearable electronics. Therefore, how to prepare highly stretchable and continuously spinnable PEDOT:PSS-based conductive fibers has become a hot research topic in the current scientific research field at home and abroad. Summary of the invention

[0003] The purpose of the present invention is to provide a spinning technology for high-elongation PEDOT:PSS / PEG conductive fibers to solve the problems of low stretchability and poor conductive stability in the current wet spinning technology, so as to expand the application of fibers in the field of wearable electronics.

[0004] The spinning technology scheme of the present invention is as follows:

[0005] A spinning technology for high-elongation PEDOT:PSS / PEG conductive fibers, characterized in that the preparation steps include:

[0006] S1. Prepare a PEDOT:PSS mixed spinning solution at room temperature, add PEG solid particles and DMSO solvent to the spinning solution, stir mechanically for 2-3 hours, and obtain a blended spinning solution after ultrasonic defoaming;

[0007] S2, the blended spinning solution is vertically and uniformly pumped into a mixed coagulation bath through a uniaxial spinning needle by a syringe pump, the mixed coagulation bath is a mixed solution of ethanol, water, copper chloride and lithium chloride, the blended spinning solution is solidified in the mixed coagulation bath, and then enters the EG bath and is washed and collected;

[0008] S3. The collected fibers were heated in a vacuum drying oven at 50° C. for 3 h, and finally highly stretched PEDOT:PSS / PEG conductive fibers were obtained.

[0009] Further, in S1, preparing the mixed spinning solution at room temperature means concentrating the PEDOT:PSS aqueous solution purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd. to 18-23 mg / mL. Further, in S1, the mass of PEG accounts for 5%-20% of the total mass of the mixed spinning solution, and the mass of DMSO accounts for 3%-10% of the total mass of the mixed spinning solution.

[0010] Furthermore, in S1, ultrasonic defoaming refers to ultrasonic dispersion for 30 minutes, with an ultrasonic oscillation frequency of 40 KHz, and then standing still after uniform dispersion to obtain a uniform blended spinning solution.

[0011] Furthermore, in S2, the volume ratio of water to ethanol in the mixed coagulation bath is 7:3.

[0012] Furthermore, in S2, in the mixed coagulation bath, Cu 2+ The concentration is 0.2 mol / L, Li + The concentration is 0.1mol / L.

[0013] Furthermore, the needle of the uniaxial spinning needle in S2 is 25G.

[0014] Furthermore, the washed fibers in S2 are collected by external winding using a polytetrafluoroethylene rod.

[0015] The beneficial effects of the present invention are:

[0016] 1. The present invention introduces water-soluble polymer PEG and DMSO into the spinning solution to prepare PEDOT:PSS / PEG conductive fibers with high tensile properties and excellent performance. DMSO is a common polar organic solvent additive, which can remove the insulating PSS chain to a certain extent, enhance the conductivity of PEDOT:PSS, and is used to adjust the PEDOT conformation in the spinning preparation. The addition of DMSO helps to improve the spinnability of the fiber, making the PEDOT:PSS molecules and PEG molecules more tightly entangled, which is manifested in the disappearance of surface cracks and the improvement of tensile properties on a macro scale.

[0017] 2. The spinning technology of the present invention is continuously prepared by uniaxial wet spinning technology, and the coagulation bath uses an environmentally friendly water and ethanol mixed coagulation bath, and Cu is added to the coagulation bath. 2+ , Li + , Cu 2+ and Li + The spinning solution is rapidly fiberized through electrostatic complexation. As an auxiliary molding additive, it shortens the conjugated structure of the PEDOT molecular main chain and increases entanglement, thereby promoting the formation of a stable PEDOT:PSS / PEG cross-linked network, which significantly improves the stretchability and conductivity of the fiber.

[0018] 3. The present invention adopts wet spinning technology to prepare fibers, by adding Cu 2+ , Li 2+ Auxiliary molding improves stretchability, and EG post-treatment improves conductivity. The excellent performance makes this fiber a functional material with important development potential in the field of flexible electronic devices. DETAILED DESCRIPTION

[0019] In order to more clearly illustrate the technical means, innovative features, objectives and effects achieved by the present invention, the present invention will be explained in detail with reference to specific examples.

[0020] The PEDOT:PSS of the present invention is poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate); PEG is polyethylene glycol; DMSO is dimethyl sulfoxide; and EG is ethylene glycol.

[0021] It should be noted that the PEDOT:PSS aqueous solution was provided by Sigma-Aldrich (Shanghai) Trading Co., Ltd. with a mass concentration of 13 mg / mL. The molecular weight of PEG used was 4000 and was purchased from Aladdin Reagent (Shanghai) Co., Ltd. Ethylene glycol (EG, AR) and dimethyl sulfoxide (DMSO, AR) were purchased from Aladdin Reagent (Shanghai) Co., Ltd. Copper chloride (CuCl2, AR) and lithium chloride (LiCl, AR) were purchased from Sinopharm Chemical Reagent Co., Ltd.

[0022] Example 1

[0023] A spinning technology for highly stretchable PEDOT:PSS / PEG conductive fibers comprises the following steps:

[0024] S1. Take a certain volume of 13 mg / mL PEDOT:PSS aqueous solution, concentrate it to 23 mg / mL PEDOT:PSS solution by heating and stirring, add PEG solid particles and DMSO solvent thereto, the mass of PEG accounts for 15% of the total mass of the blended spinning solution, the mass of DMSO accounts for 5% of the total mass of the blended spinning solution, stir the blended solution continuously at room temperature for 3 hours to fully mix, then place the mixed solution in an ultrasonic oscillator with an operating frequency of 40KHz for 30 minutes, evenly disperse it, and then let it stand for defoaming to obtain a uniform blended spinning solution;

[0025] S2, the blended spinning solution was vertically and uniformly pumped into the mixed coagulation bath by a syringe pump through a uniaxial spinning needle (needle head 25G), the injection speed was 0.2mL / min, the mixed coagulation bath was a mixed solution of ethanol, water, copper chloride, and lithium chloride, the volume ratio of ethanol to water was 7:3, Cu 2+ The added concentration is 0.2 mol / L, Li +The added concentration is 0.1 mol / L. After the blended spinning solution is solidified in a mixed coagulation bath, it enters an EG bath and then is washed. The washed fibers are collected by external winding with a polytetrafluoroethylene rod.

[0026] S3, heating the collected fibers in a vacuum drying oven at 50°C for 3 hours, and finally obtaining PEDOT:PSS / PEG conductive fibers with a high tensile elongation ratio. The PEDOT:PSS / PEG conductive fibers spun in this example have a tensile elongation ratio of 85.0% and a conductivity of 6.54 S / cm.

[0027] Example 2

[0028] A spinning technology for highly stretchable PEDOT:PSS / PEG conductive fibers comprises the following steps:

[0029] S1. Take a certain volume of 13 mg / mL PEDOT:PSS aqueous solution, concentrate it to 20 mg / mL PEDOT:PSS solution by heating and stirring, add PEG solid particles and DMSO solvent thereto, the mass of PEG accounts for 10% of the total mass of the blended spinning solution, and the mass of DMSO accounts for 5% of the total mass of the blended spinning solution, stir the blended solution continuously at room temperature for 2 hours to fully mix, then place the mixed solution in an ultrasonic oscillator with an operating frequency of 40KHz for 30 minutes, evenly disperse it, and then let it stand for defoaming to obtain a uniform blended spinning solution;

[0030] S2, the blended spinning solution was vertically and uniformly pumped into the mixed coagulation bath by a syringe pump through a uniaxial spinning needle (needle head 25G), the injection speed was 0.2mL / min, the mixed coagulation bath was a mixed solution of ethanol, water, copper chloride, and lithium chloride, the volume ratio of ethanol to water was 7:3, Cu 2+ The added concentration is 0.2 mol / L, Li + The added concentration is 0.1 mol / L. After the blended spinning solution is solidified in a coagulation bath, it enters an EG bath and then is washed. The washed fibers are collected by external winding with a polytetrafluoroethylene rod.

[0031] S3, the collected fibers were heated in a vacuum drying oven at 50°C for 3 hours, and finally PEDOT:PSS / PEG conductive fibers with a high tensile elongation ratio were obtained. The PEDOT:PSS / PEG conductive fibers spun in this example had a tensile elongation of 75.0% and a conductivity of 7.08 S / cm

[0032] Example 3

[0033] A spinning technology for highly stretchable PEDOT:PSS / PEG conductive fibers comprises the following steps:

[0034] S1. Take a certain volume of 13 mg / mL PEDOT:PSS aqueous solution, concentrate it to 18 mg / mL PEDOT:PSS solution by heating and stirring, add PEG solid particles and DMSO solvent thereto, the mass of PEG accounts for 5% of the total mass of the blended spinning solution, the mass of DMSO accounts for 10% of the total mass of the blended spinning solution, stir the blended solution continuously at room temperature for 2 hours to fully mix, then place the mixed solution in an ultrasonic oscillator with an operating frequency of 40KHz for 30 minutes, evenly disperse it, and then let it stand for defoaming to obtain a uniform blended spinning solution;

[0035] S2, the blended spinning solution was vertically and uniformly pumped into the mixed coagulation bath by a syringe pump through a uniaxial spinning needle (needle head 25G), the injection speed was 0.2mL / min, the mixed coagulation bath was a mixed solution of ethanol, water, copper chloride, and lithium chloride, the volume ratio of ethanol to water was 7:3, Cu 2+ The added concentration is 0.2 mol / L, Li + The added concentration is 0.1 mol / L. After the blended spinning solution is solidified in a coagulation bath, it enters an EG bath and then is washed. The washed fibers are collected by external winding with a polytetrafluoroethylene rod.

[0036] S3, heating the collected fibers in a vacuum drying oven at 50°C for 3 hours, and finally obtaining PEDOT:PSS / PEG conductive fibers with a high tensile elongation ratio. The PEDOT:PSS / PEG conductive fibers spun in this example have a tensile elongation of 68.0% and a conductivity of 7.43 S / cm.

[0037] Example 4

[0038] A spinning technology for highly stretchable PEDOT:PSS / PEG conductive fibers comprises the following steps:

[0039] S1. Take a certain volume of 13 mg / mL PEDOT:PSS aqueous solution, concentrate it to 23 mg / mL PEDOT:PSS solution by heating and stirring, add PEG solid particles and DMSO solvent thereto, the mass of PEG accounts for 20% of the total mass of the blended spinning solution, and the mass of DMSO accounts for 3% of the total mass of the blended spinning solution, stir the blended solution continuously at room temperature for 3 hours to fully mix, then place the mixed solution in an ultrasonic oscillator with an operating frequency of 40KHz for 30 minutes, evenly disperse it, and then let it stand for defoaming to obtain a uniform blended spinning solution;

[0040] S2, the blended spinning solution was vertically and uniformly pumped into the mixed coagulation bath by a syringe pump through a uniaxial spinning needle (needle head 25G), the injection speed was 0.2mL / min, the mixed coagulation bath was a mixed solution of ethanol, water, copper chloride, and lithium chloride, the volume ratio of ethanol to water was 7:3, Cu 2+The added concentration is 0.2 mol / L, Li + The added concentration is 0.1 mol / L. After the blended spinning solution is solidified in a coagulation bath, it enters an EG bath and then is washed. The washed fibers are collected by external winding with a polytetrafluoroethylene rod.

[0041] S3, heating the collected fibers in a vacuum drying oven at 50°C for 3 hours, and finally obtaining PEDOT:PSS / PEG conductive fibers with a high tensile elongation ratio. The PEDOT:PSS / PEG conductive fibers spun in this example have a tensile elongation of 73.0% and a conductivity of 5.72 S / cm.

[0042] Comparative Example 1

[0043] Only 15% of PEG solid particles were added to the blended spinning solution of S1, and no DMSO solvent was added. The other conditions were the same as those of Example 1. The PEDOT:PSS / PEG conductive fiber spun in this comparative example had a tensile elongation of 70.0% and a conductivity of 5.60 S / cm.

[0044] Comparative Example 2

[0045] Only 5% DMSO solvent was added to the blended spinning solution of S1, and no PEG solid particles were added. The rest was the same as Example 1. The PEDOT:PSS conductive fiber spun in this comparative example had a tensile elongation of 63.0% and a conductivity of 6.30 S / cm.

[0046] Comparative Example 3

[0047] After the blended spinning solution of S2 was solidified in a coagulation bath, it was directly washed with water without entering the EG bath. Others were the same as in Example 1. The PEDOT:PSS / PEG conductive fiber spun in this comparative example had a tensile elongation of 78.0% and a conductivity of 5.21 S / cm.

[0048] Comparative Example 4

[0049] The mixed coagulation bath of S2 is a mixed solution of ethanol and water, without adding Cu 2+ , Li + The other conditions are the same as those in Example 1. The PEDOT:PSS / PEG conductive fiber spun in this comparative example has a tensile elongation of 72% and a conductivity of 5.59 S / cm.

[0050] By comparing Example 1 and Comparative Example 1, it is found that after a small amount of DMSO solvent is added to the spinning solution, the conductivity of the fiber is significantly increased, indicating that DMSO removes the insulating PSS chain to a certain extent, causing the PEDOT structure to undergo a benzoquinone structure transformation, thereby improving the conductivity of the fiber. By comparing Example 1 and Comparative Example 2, it is found that after PEG is added to the original spinning solution, the tensile strength and conductivity of the fiber are improved. By comparing Example 1 and Comparative Example 3, it is found that the conductivity of the fiber is significantly improved after post-treatment with an EG bath, indicating that EG can remove excess PSS and non-conductive components to improve the conductivity of the fiber. By comparing Example 1 and Comparative Example 4, it is found that the metal salt Cu doped in the fiber 2+ and Li + It can improve the stretchability and conductivity, and improve the spinnability of the fiber. This is because the metal ions, as auxiliary molding additives, shorten the conjugated structure of the PEDOT molecule main chain and increase entanglement, thereby promoting the formation of a stable PEDOT:PSS / PEG cross-linked network, which significantly improves the stretchability and conductivity of the fiber.

Claims

1. A spinning technology for high elongation PEDOT:PSS / PEG conductive fibers, It is characterized in that The preparation steps include: S1. Prepare a PEDOT:PSS mixed spinning solution at room temperature, add PEG solid particles and DMSO solvent to the spinning solution, stir mechanically for 2-3 hours, and obtain a blended spinning solution after ultrasonic defoaming; S2, the blended spinning solution is vertically and uniformly pumped into a mixed coagulation bath through a uniaxial spinning needle by a syringe pump, the mixed coagulation bath is a mixed solution of ethanol, water, copper chloride and lithium chloride, the blended spinning solution is solidified in the mixed coagulation bath, and then enters the EG bath and is washed and collected; S3. The collected fibers were heated in a vacuum drying oven at 50° C. for 3 h, and finally highly stretched PEDOT:PSS / PEG conductive fibers were obtained.

2. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that In S1, preparing the mixed spinning solution at room temperature refers to concentrating the PEDOT:PSS aqueous solution purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd. to 18-23 mg / mL.

3. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that The mass of PEG in S1 accounts for 5%-20% of the total mass of the blended spinning solution, and the mass of DMSO accounts for 3%-10% of the total mass of the blended spinning solution.

4. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that In S1, ultrasonic defoaming refers to ultrasonic dispersion for 30 minutes, with an ultrasonic oscillation frequency of 40 KHz, and then standing still after uniform dispersion to obtain a uniform blended spinning solution.

5. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that In S2, the volume ratio of water to ethanol in the mixed coagulation bath is 7:

3.

6. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that S2, mixed coagulation bath, Cu 2+ The concentration is 0.2 mol / L, Li + The concentration is 0.1mol / L.

7. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that The needle of the uniaxial spinning needle in S2 is 25G.

8. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that The EG bath in S2 is EG and water in a volume ratio of 1:

1.

9. The spinning technology of a high elongation PEDOT:PSS / PEG conductive fiber according to claim 1, It is characterized in that The washed fibers in S2 were collected by external winding using a polytetrafluoroethylene rod.