Durability test method for tire bead of radial tire
By setting appropriate crown arc, load and air pressure in bead durability test, a more accurate bead durability evaluation is achieved, and the problems of long test time, high cost and inconsistent damage form in the prior art are solved. The market demand for high load-bearing and high-speed performance.
Patent Information
- Application Number
- CN202411122770.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-08
AI Technical Summary
The existing bead durability test methods cannot effectively evaluate the durability of tires under high load-bearing and high-speed performance. The test time is long and the cost is high, and the damage form is different from that in actual use, so it cannot meet the rapid development of tires in the market. need.
A radial tire bead durability test method is adopted, including grinding the tread before the test, setting the crown arc to be no less than 580mm, installing it on the measuring rim, and conducting the test under a 38℃ environment after inflation. The test procedure is divided into two sections , the load gradually increases to 2.1-2.5 times the standard load, the speed remains 40-50km/h, and the air pressure remains 900-1000kPa, shortening the test time and improving the test accuracy.
Shorten the test time, avoid damage to non-bead parts, improve the test accuracy, and make the tire damage the same as in actual use, effectively evaluate the durability of the bead and adapt to the market's requirements for high load-bearing and high-speed performance. , reducing the cost of testing.
Smart Images

Figure CN118913723A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tire bead durability evaluation, and in particular to a radial tire bead durability test method. Background Art
[0002] With the construction of expressways in my country, the speed of vehicles is getting faster and faster, and the high-speed performance of tires needs to be improved. In the past two years, the high-horsepower engines of automobiles have been continuously developed: the horsepower of automobiles has increased from 420PS to 560PS, and now there are even vehicles with horsepower of more than 700PS. This requires tires to have not only high load-bearing rate, but also faster vehicle speeds. Tires with high load-bearing rate and high-speed performance.
[0003] This poses a challenge to the tire bead performance durability test method. Due to changes in the market use environment, the existing tire bead durability test method for load-bearing performance can no longer adapt to the changing use environment.
[0004] Market research has found that many regions require both heavy-load and high-speed performance, which requires both high load rate and high speed. Therefore, we are required to adapt to the development of the market environment when evaluating the tire bead durability machine test. Now the tire use environment has undergone tremendous changes. The durability test for evaluating the tire bead performance can no longer objectively evaluate whether the product can meet the market, and the damage form of the tire in the existing test method is very different from the damage form in actual use.
[0005] For example, the name is a test method for the durability performance of the bead of a truck tire, and the application number is CN111929081A. The tread is polished before the tire is assembled, and the tread is polished to the bottom of the tire groove. The polished test tire is installed on a measuring rim that meets the requirements, and is inflated with a test pressure of 1100kPa. After inflation, the test tire is parked at an ambient temperature of 38℃±3℃ for no less than 3h; the test is carried out: the test procedure is set up in 2 stages, the first stage lasts for 2h, and the pressure is set to the standard load pressure; the second stage runs until the tire is damaged, and the pressure is set to 200% of the standard load pressure; the speed is kept unchanged at 50km / h during the test. The speed of this test method meets the current high-speed performance of tires, but the load rate and air pressure do not meet the requirements of the existing tire performance, which makes the test running time of the modified test method longer and the test cost higher. In the existing bead durability test, the evaluation methods of various manufacturers are different due to different test conditions, and the differences lie in air pressure, load rate, and speed. The existing tire bead durability test method for evaluating tire load-bearing performance cannot effectively evaluate tire bead durability performance, either because the tire has been running for too long or the tire is damaged at the shoulder. It can only evaluate tires with a load-bearing rate below 180%, and cannot meet the current market requirements for tires. Summary of the invention
[0006] The technical problem to be solved by the present invention is how to effectively evaluate the test method required by the existing market for tires.
[0007] The present invention solves the above technical problems through the following technical means:
[0008] The present invention provides a radial tire bead durability test method, comprising the following steps:
[0009] The tread of the test tire shall be polished before assembly, and the tread shall be polished to a crown curvature of not less than 580mm;
[0010] Install the polished test tire on a measuring rim that meets the requirements and inflate it with a test pressure of 1100kPa. After inflation, leave the test tire at an ambient temperature of 38±3℃ for no less than 3h;
[0011] Test: The test procedure is set up in 2 stages. The first stage lasts for 3 hours, and the load is set to 1.5 times the standard load pressure; the second stage runs until the tire is damaged, and the load is set to 2.1-2.5 times the standard load pressure; during the test, the speed remains unchanged at 40-50km / h, and the air pressure remains unchanged at 900-1000kpa.
[0012] Beneficial effects: The test method of the present invention further shortens the test time and avoids the premature damage of non-bead parts during the test, which cannot effectively evaluate the durability of the bead. In addition, the tire damage form of the test method of the present invention is the same as the actual damage form, indicating that the test method of the present invention has high accuracy.
[0013] Preferably, when the test tire has an inner tube, the test speed is unchanged at 40 km / h.
[0014] Preferably, when the test tire is tubeless, the test speed is unchanged at 50 km / h.
[0015] Preferably, the air pressure is 900 kPa constant.
[0016] Preferably, the air pressure is constant at 1000 kPa.
[0017] Preferably, the crown curvature is 600-800 mm.
[0018] More preferably, the crown curvature is 600-650 mm.
[0019] Preferably, the test tire is at an ambient temperature of 38°C.
[0020] Preferably, the parking time is 4 hours.
[0021] The advantages of the present invention are:
[0022] Compared with the existing tire bead durability test method, the tread is firstly polished and the crown curvature is ensured to be above 680mm, which further shortens the test operation time and reduces the test cost; secondly, the test method of the present invention adopts two speeds according to market demand and tire performance, which is aimed at test tires with or without inner tubes, and the speeds adopted are all the highest speeds of the test tires, which can effectively evaluate the tire bead durability performance; thirdly, different loads are adopted according to market positioning to effectively evaluate product performance and avoid waste caused by excessive tire product performance; fourthly, the tire pressure is adopted according to the characteristics of different tire specifications and load-bearing rate performance. Use different air pressures to avoid low air pressure, which may cause tire rolling, shoulder void and tire cracking. Fifth, and most importantly, the tire bead durability test method for heavy-load products improves the test speed, load and tire pressure, and adapts to the actual use environment of high-horsepower and fast transportation. The average test running time of the test method of the present invention is 30-70h, during which the performance of different tires can be well distinguished. A running time of less than 30h indicates that the performance of the tire does not meet market requirements, and a running time of more than 70h indicates that the test time is long, which is not conducive to cost control for the test manufacturer, and the test cost is high and has no practicality. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a picture of the test tire before grinding in the embodiment;
[0024] Figure 2 This is a picture of the test tire after grinding in the embodiment;
[0025] Figure 3 are pictures showing the damage of the test tires in Example 1, wherein a represents SDM318, b represents TA665N, c represents JX359H1, and d represents WGC29;
[0026] Figure 4 This is a picture showing the damage of the test tire in Example 2. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0029] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0030] Example 1
[0031] This embodiment provides a radial tire bead durability test method, which specifically includes the following steps:
[0032] Preparation before the test:
[0033] Grind the tread of the test tire before assembly until the crown curvature is not less than 580mm. Figure 2 As shown, the polished test tire is then mounted on a measuring rim that meets the requirements and inflated with a test air pressure of 1100 kPa. After inflation, the test tire is placed at an ambient temperature of 38°C for 4 hours until the test tire is stable.
[0034] Test stage: The test tire used in this embodiment has a specification of 13R22.5 and is tubeless.
[0035] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 50km / h, and the test air pressure remains unchanged at 1000kpa.
[0036] Stage 2: Set the test tire load to 2.3 times the standard load pressure, keep the test speed at 50km / h, and keep the test air pressure at 1000kpa until the test tire is damaged. Figure 3 The results of the test in this embodiment are shown in Table 1.
[0037] Example 2
[0038] This embodiment provides a radial tire bead durability test method, which specifically includes the following steps:
[0039] Preparation before the test:
[0040] Grind the tread of the test tire before assembly until the crown curvature is not less than 580mm. Then install the ground test tire on a measuring rim that meets the requirements and inflate it with a test pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38℃ for 4 hours until the test tire is stable.
[0041] Test stage: The test tire used in this embodiment has a specification of 12R22.5 and is tubeless.
[0042] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 50km / h, and the test air pressure remains unchanged at 900kpa.
[0043] Stage 2: Set the test tire load to 2.1 times the standard load pressure, keep the test speed at 50km / h, and keep the test air pressure at 900kpa until the test tire is damaged. Figure 4 The results of the test in this embodiment are shown in Table 1.
[0044] Example 3
[0045] This embodiment provides a radial tire bead durability test method, which specifically includes the following steps:
[0046] Preparation before the test:
[0047] Grind the tread of the test tire before assembly until the crown curvature is not less than 580mm. Then install the ground test tire on a measuring rim that meets the requirements and inflate it with a test pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38℃ for 4 hours until the test tire is stable.
[0048] Test stage: The test tire used in this embodiment has a specification of 12R20 and an inner tube.
[0049] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 40km / h, and the test air pressure remains unchanged at 1000kpa.
[0050] Stage 2: The load of the test tire is set to 2.3 times the standard load pressure, the test speed is kept constant at 40 km / h, and the test air pressure is kept constant at 1000 kPa until the test tire is damaged. The test results of this embodiment are shown in Table 1.
[0051] Example 4
[0052] This embodiment provides a radial tire bead durability test method, which specifically includes the following steps:
[0053] Preparation before the test:
[0054] Grind the tread of the test tire before assembly until the crown curvature is not less than 580mm. Then install the ground test tire on a measuring rim that meets the requirements and inflate it with a test pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38℃ for 4 hours until the test tire is stable.
[0055] Test stage: The test tire used in this embodiment has a specification of 12R20 and an inner tube.
[0056] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 40km / h, and the test air pressure remains unchanged at 1000kpa.
[0057] Stage 2: The load of the test tire is set to 2.5 times the standard load pressure, the test speed is kept constant at 40 km / h, and the test air pressure is kept constant at 1000 kPa until the test tire is damaged. The experimental results of this embodiment are shown in Table 1.
[0058] Comparative Example 1
[0059] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0060] Preparation before the test:
[0061] Grind the tread of the test tire before assembly until the crown curvature is 610mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38°C for 4 hours until the test tire is stable.
[0062] Test stage: The test tire used in this embodiment has a specification of 13R22.5 and is tubeless.
[0063] Phase 1: Set the load of the test tire to the standard load pressure, the test time is 2 hours, the test speed remains unchanged at 30km / h, and the test air pressure remains unchanged at 650kpa.
[0064] Stage 2: The load of the test tire is set to 2 times the standard load pressure, the test speed is kept constant at 30 km / h, and the test air pressure is kept constant at 650 kPa until the test tire is damaged. The experimental results of this embodiment are shown in Table 1.
[0065] Comparative Example 2
[0066] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0067] Preparation before the test:
[0068] Grind the tread of the test tire before assembly until the crown curvature is 610mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38°C for 4 hours until the test tire is stable.
[0069] Test stage: The test tire used in this embodiment has a specification of 13R22.5 and is tubeless.
[0070] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 50km / h, and the test air pressure remains unchanged at 650kpa.
[0071] Stage 2: The load of the test tire is set to 2.3 times the standard load pressure, the test speed is kept constant at 50 km / h, and the test air pressure is kept constant at 650 kPa until the test tire is damaged. The results of this comparative test are shown in Table 1.
[0072] Comparative Example 3
[0073] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0074] Preparation before the test:
[0075] Grind the tread of the test tire before assembly until the crown curvature is 610mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38°C for 4 hours until the test tire is stable.
[0076] Test stage: The test tire used in this embodiment has a specification of 13R22.5 and is tubeless.
[0077] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 30km / h, and the test air pressure remains unchanged at 1000kpa.
[0078] Stage 2: The load of the test tire is set to 2.3 times the standard load pressure, the test speed is kept constant at 30 km / h, and the test air pressure is kept constant at 1000 kPa until the test tire is damaged. The results of this comparative test are shown in Table 1.
[0079] Comparative Example 4
[0080] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0081] Preparation before the test:
[0082] Grind the tread of the test tire before assembly until the crown curvature is 610mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38°C for 4 hours until the test tire is stable.
[0083] Test stage: The test tire used in this embodiment has a specification of 13R22.5 and is tubeless.
[0084] Phase 1: Set the load of the test tire to the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 50km / h, and the test air pressure remains unchanged at 1000kpa.
[0085] Stage 2: The load of the test tire is set to 2 times the standard load pressure, the test speed is kept constant at 50 km / h, and the test air pressure is kept constant at 1000 kPa until the test tire is damaged. The results of this comparative test are shown in Table 1.
[0086] Comparative Example 5
[0087] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0088] Preparation before the test:
[0089] Grind the tread of the test tire before assembly until the crown curvature is 600mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38°C for 4 hours until the test tire is stable.
[0090] Test stage: The test tire used in this embodiment has a specification of 12R22.5 and is tubeless.
[0091] Phase 1: Set the load of the test tire to the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 50km / h, and the test air pressure remains unchanged at 900kpa.
[0092] Stage 2: The load of the test tire is set to 2 times the standard load pressure, the test speed is kept constant at 50 km / h, and the test air pressure is kept constant at 900 kPa until the test tire is damaged. The experimental results of this comparative example are shown in Table 1.
[0093] Comparative Example 6
[0094] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0095] Preparation before the test:
[0096] Grind the tread of the test tire before assembly until the crown curvature is 650mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38℃ for 4 hours until the test tire is stable.
[0097] Test stage: The test tire used in this embodiment has a specification of 12R20 and an inner tube.
[0098] Phase 1: Set the load of the test tire to the standard load pressure, the test time is 2 hours, the test speed remains unchanged at 30km / h, and the test air pressure remains unchanged at 600kpa.
[0099] Stage 2: The load of the test tire is set to 2 times the standard load pressure, the test speed is kept constant at 30 km / h, and the test air pressure is kept constant at 600 kPa until the test tire is damaged. The experimental results of this comparative example are shown in Table 1.
[0100] Comparative Example 7
[0101] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0102] Preparation before the test:
[0103] Grind the tread of the test tire before assembly until the crown curvature is 650mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38℃ for 4 hours until the test tire is stable.
[0104] Test stage: The test tire used in this embodiment has a specification of 12R20 and an inner tube.
[0105] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 40km / h, and the test air pressure remains unchanged at 600kpa.
[0106] Stage 2: The load of the test tire is set to 2.3 times the standard load pressure, the test speed is kept constant at 40 km / h, and the test air pressure is kept constant at 600 kPa until the test tire is damaged. The experimental results of this comparative example are shown in Table 1.
[0107] Comparative Example 8
[0108] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0109] Preparation before the test:
[0110] Grind the tread of the test tire before assembly until the crown curvature is 650mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38℃ for 4 hours until the test tire is stable.
[0111] Test stage: The test tire used in this embodiment has a specification of 12R20 and an inner tube.
[0112] Phase 1: Set the load of the test tire to 1.5 times the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 50km / h, and the test air pressure remains unchanged at 1000kpa.
[0113] Stage 2: The load of the test tire is set to 2.3 times the standard load pressure, the test speed is kept constant at 50 km / h, and the test air pressure is kept constant at 1000 kPa until the test tire is damaged. The experimental results of this comparative example are shown in Table 1.
[0114] Comparative Example 9
[0115] This comparative example provides a radial tire bead durability test method, which specifically includes the following steps:
[0116] Preparation before the test:
[0117] Grind the tread of the test tire before assembly until the crown curvature is 650mm. Then mount the grinded test tire on a measuring rim that meets the requirements and inflate it with a test air pressure of 1100kPa. After inflation, place the test tire at an ambient temperature of 38℃ for 4 hours until the test tire is stable.
[0118] Test stage: The test tire used in this embodiment has a specification of 12R20 and an inner tube.
[0119] Phase 1: Set the load of the test tire to the standard load pressure, the test time is 3 hours, the test speed remains unchanged at 40km / h, and the test air pressure remains unchanged at 1000kpa.
[0120] Stage 2: The load of the test tire is set to 2 times the standard load pressure, the test speed is kept constant at 40 km / h, and the test air pressure is kept constant at 1000 kPa until the test tire is damaged. The experimental results of this comparative example are shown in Table 1.
[0121] Experimental Example: The experimental results of the tires of the embodiment and the comparative example are recorded as follows:
[0122] Table 1 Experimental results of tires tested in the embodiment and comparative example
[0123]
[0124]
[0125] The test time should be neither too long nor too short. If the test time is too long, it will not only increase the test cost, but also make it impossible to distinguish the performance of the tires; if the test time is too short, the performance of the test tires cannot be distinguished, which does not meet the test and market needs. The test time is appropriate between 30-70h, with appropriate test costs and appropriate test tire performance.
[0126] Speed selection of the present invention: Most of the existing technologies are 30km / h. With the increase of vehicle horsepower, the speed of 30km / h cannot meet the requirements of actual use. The present invention has different specifications and different test speeds. The speed of the inner tube is lower at 40km / h, and the speed of the tubeless tire is lower in heat generation and can reach 50km / h; for example, when the speed of 13R22.5 reaches 50km / h, the tire running time can reach 33 hours.
[0127] The air pressure selection of the present invention: Most of the existing technologies are 600-650kpa, which is prone to shoulder voids and cannot effectively evaluate the tire bead durability performance. The present invention adjusts the air pressure to be based on the specification classification and the safety of indoor machine tool testing. The air pressure cannot exceed 1000kpa. The test pressure of the small specification 12R22.5 is 900kpa; the test pressure of the large specification 12R20 / 13R22.5 is 1000kpa. The test method of the present invention will not cause shoulder voids, and the tire damage form is the same as the actual damage form in use, which meets market demand.
[0128] Load selection of the present invention: Most of the existing technologies are standard load and twice the standard load. The present invention sets different loads according to different positioning and specifications, so as to achieve accurate evaluation and avoid the problem of serious overperformance in evaluating tires.
[0129] As shown in Table 1, compared with the comparative example, the comparative example has too large a sinking amount of the test tire, resulting in excessive shear force at the end of the belt layer, cracks, and the extension of the cracks leads to shoulder space. Compared with the test method of the comparative example, the test method of the present invention has a higher load and a higher speed. The tire bead not only bears a high load, high deformation, and high strain, but also generates a lot of heat due to the increased speed, and the physical and mechanical properties of the tire components are greatly reduced, so the test running time is greatly reduced.
[0130] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A radial tire bead durability test method, characterized in that: The following steps are involved: The tread of the test tire shall be polished before assembly, and the tread shall be polished to a crown curvature of not less than 580mm; Install the polished test tire on a measuring rim that meets the requirements and inflate it with a test pressure of 1100kPa. After inflation, leave the test tire at an ambient temperature of 38±3℃ for no less than 3h; Test: The test procedure is set up in 2 stages. The first stage lasts for 3 hours, and the load is set to 1.5 times the standard load pressure; the second stage runs until the tire is damaged, and the load is set to 2.1-2.5 times the standard load pressure; during the test, the speed is maintained at 40-50km / h and the air pressure is maintained at 900-1000kpa.
2. The radial tire bead durability test method according to claim 1, characterized in that: When the test tire has an inner tube, the test speed remains unchanged at 40 km / h.
3. The radial tire bead durability test method according to claim 1, characterized in that: When the test tire has no inner tube, the test speed is 50 km / h unchanged.
4. The radial tire bead durability test method according to claim 1, characterized in that: The air pressure is constant at 900 kPa.
5. The radial tire bead durability test method according to claim 1, characterized in that: The air pressure is constant at 1000 kPa.
6. The radial tire bead durability test method according to claim 1, characterized in that: The test tires were at an ambient temperature of 38°C.
7. The radial tire bead durability test method according to claim 1, characterized in that: The parking time is 4 hours.
8. The radial tire bead durability test method according to claim 1, characterized in that: The camber of the tire crown is 600-800 mm.
9. The radial tire bead durability test method according to claim 1, characterized in that: The crown curvature is 600-650mm.
Citation Information
Patent Citations
Indoor evaluation method for shoulder separation fault of all-steel radial tire
CN109238748A
Method for testing durability of truck tire bead
CN111929081A
Method for testing scratch resistance of car tire
CN113465948A
Tire bead durability test method
CN117433806A
Durability testing method for pneumatic tire
JP2010133796A