Method for testing strength of needle coke particles
By adopting testing instruments and equipment conforming to the T/ZGTS 002-2022 standard, and combining them with specific sieving times, the accuracy of needle coke particle strength testing was solved, ensuring the accuracy of the formulation during production and improving the performance of carbon products and graphite.
Patent Information
- Application Number
- CN202411053261.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies make it difficult to accurately distinguish the strength of different particles when testing the strength of needle coke particles, leading to formula distortion during production and inaccurate test results.
Using testing instruments and equipment conforming to the T/ZGTS 002-2022 standard, combined with specific sieving time and strength calculation methods, two sets of particle strength coefficients were obtained through 1-minute and 3-minute sieving. When the difference was 3%-4%, high-quality needle coke was determined for use in the production of carbon products or graphite.
It enables accurate differentiation of the strength of needle coke particles, ensures the accuracy of the formula during the production process, and improves the mechanical and electrical properties of subsequent carbon products and graphite.
Abstract
Description
Technical Field
[0001] The invention relates to a performance testing technology for inorganic non-metallic materials. Background Art
[0002] The working principle of the particle strength tester is to use compression testing to determine the strength of particles. The particles to be tested are placed in a container and a compression force perpendicular to the surface of the particles is applied. The deformation and breaking force of the particles under a certain compression force are measured to calculate the strength of the particles.
[0003] In the compression test, the particles to be tested are placed between two parallel plates, and then a certain pressure is applied to measure the deformation and breaking force of the particles. Based on the measured data, the strength of the particles can be calculated, including crushing strength, bending strength, etc. The strength of the particles is not only related to the composition and structure of the particles, but also to factors such as the particle size and surface morphology. Therefore, when conducting a particle strength test, it is necessary to select appropriate test conditions and test methods to ensure the accuracy and reliability of the test results.
[0004] In the industry group standard TZGTS002-2019 "Oil-based Needle Coke for Graphite Electrodes", the particle strength coefficient is a measure of the ability of carbon material particles to resist crushing. A specified amount of coke particles in a specified size range are pressurized using a standard test method, and the ratio of the number of uncrushed particles to the original weight of the sample is expressed as a percentage. Summary of the invention
[0005] Purpose of the invention: Provided is a test method for the strength of needle coke particles, which has relatively stable particle quality and is not easily destroyed during post-production use.
[0006] Technical solution: The test method for the needle coke particle strength of the present invention adopts the following test instruments and equipment recommended by the T / ZGTS 002-2022 standard: 1 Universal material testing machine: range 0~300 kN, accuracy no more than 1%.
[0007] 2 Mechanical vibration standard screening machine.
[0008] 3 Balance: sensitivity 0.1 g.
[0009] 4 Jaw crusher or roll crusher.
[0010] 5. Stopwatch.
[0011] 6. Mold: Material: 45 #Steel; height 120 mm, inner diameter 60 mm, outer diameter 140 mm; upper gasket material is bakelite, Φ60 mm×20 mm; lower gasket material is 45 # steel.
[0012] The T / ZGTS 002-2022 standard does not specify the screening time of the sample. The present invention imposes the following restrictions on the screening time of needle coke: After 1 minute (10 seconds tolerance, the same below) screening and 3 minutes screening respectively (if 1 minute and 2 minutes are selected, the interval time is not enough, and a small amount of particles with natural cracks may produce broken materials, and the strength of the later products is not enough; if 1 minute and 4 minutes are selected, the particles after 3 minutes will have almost no natural cracks, and the contribution to the strength of the product will not increase much, and the qualified particles may increase artificial oscillation cracks, the qualified rate will drop a lot, causing unnecessary waste). When 1 minute screening and 3 minutes screening, take 4mm~2mm coke particles, use the quartering method to reduce to about 250g, and the sample purity requirement is not less than 95%. The specific test steps are as follows: 1. After a batch of calcined needle coke is naturally cooled, it is crushed to less than 10 mm and a portion of needle coke weighing about 1 kg is selected.
[0013] Perform 1 minute of screening, take 4mm to 2mm coke particles, and reduce them to about 250g using the quartering method. The sample purity is required to be no less than 95%, and the first particle strength coefficient is obtained by testing.
[0014] 2. From the same batch of needle coke, select another part of needle coke (about 1 kg); perform 3 minutes of screening, take out 4mm-2mm coke particles, and reduce them to about 250g by quartering method. The purity of the sample is required to be not less than 95%, and test to obtain the second particle strength coefficient.
[0015] 3. When the difference between the strength coefficient of the second particle and the strength coefficient of the first particle is concentrated at 3%-4%, needle coke is obtained, which is used to produce carbon products or graphite. At this time, the products obtained have higher mechanical strength and better quality.
[0016] When the difference between the second particle strength coefficient and the first particle strength coefficient is greater than 4%, it indicates that the particle strength is easily destroyed and the particle strength quality of the raw material is relatively poor, which will cause formulation distortion during the production batching process.
[0017] When the difference between the strength coefficient of the second particle and the strength coefficient of the first particle is less than 3%, it means that the particle strength is too large. When such needle coke particles are used to produce carbon products or graphite, the hardness is too high and the graphitization effect is not good enough. Such needle coke is not suitable for use.
[0018] The test steps for the above particle strength coefficient are: 1 Weigh 100g of the prepared sample to an accuracy of 0.1g.
[0019] 2 Place the mold on the workbench of the universal material testing machine and put the lower gasket into the bottom of the mold. Pour the weighed sample into the mold and then place the upper pressing plate on the sample.
[0020] 3. Use a Φ20 mm metal rod to hit the mold 3 to 5 times, and place the pressure rod on the upper pressure plate.
[0021] 4 Start the testing machine and slowly increase the pressure at a speed of less than 3 kN / min to 113 kN (equivalent to 40 MPa), and maintain the pressure at the specified pressure for 5 minutes.
[0022] 5 Release the pressure, take out the sample, screen and weigh the pressurized sample.
[0023] Calculation of the above particle strength coefficient: Particle strength coefficient K Calculate according to the following formula (1): ………… (1) Where: K —Particle strength coefficient, %; G —The mass of the sample on the screen after being compressed, in grams (g); G 0—The mass of the test before compression, in grams (g).
[0024] The result is the arithmetic mean of the two tests, and the test result is rounded to one decimal place (the numerical value is rounded off in accordance with the provisions of GB / T8170).
[0025] Beneficial effects: The present invention can achieve the degree of differentiation of particle strengths of various needle cokes and can more accurately evaluate the particle strengths of different needle coke raw materials.
[0026] The needle coke particles selected by the present invention have relatively good strength and quality, and will not cause formulation distortion during the production batching process. The subsequent production of carbon products or graphite has good mechanical properties such as tensile and flexural strength, compressive strength, electrical conductivity and heat transfer performance. DETAILED DESCRIPTION
[0027] The test method for the needle coke particle strength of the present application adopts the test instruments and equipment specified by the T / ZGTS 002-2022 standard to perform the following test steps: 1. After a batch of calcined needle coke is naturally cooled, all of them are crushed to less than 10 mm, and 1 kg of needle coke is selected; 1 minute of screening is performed, and needle coke particles of 4 mm to 2 mm are taken, and the particles are reduced to 250 g by quartering method, with a purity of not less than 95%, and the first particle strength coefficient is obtained by testing; 2. From the same batch of needle coke, select another part of needle coke (about 1 kg); perform sieving for 3 minutes, take coke particles of 4 mm to 2 mm, and reduce them to 250 g by quartering method, with a purity of not less than 95%, and test to obtain the second particle strength coefficient; 3. When the difference between the strength coefficient of the second particle and the strength coefficient of the first particle is 3%-4%, the obtained needle coke particles can be used for the subsequent production of high-quality graphite electrodes.
Claims
1. A method for testing the strength of needle coke particles, using the testing instrument and equipment recommended by the T / ZGTS 002-2022 standard, characterized in that: The test steps are as follows:
1. After a batch of calcined needle coke is naturally cooled, all of them are crushed to less than 10 mm, and 0.5-2 kg of needle coke is selected; 1 minute of screening is performed, and needle coke particles of 4 mm to 2 mm are taken, and the mass is reduced to about 1 / 4 by quartering method, and the first particle strength coefficient is obtained by testing; 2. From the same batch of needle coke, select another part of needle coke (about 0.5-2kg); perform sieving for 3 minutes, take out 4mm-2mm coke particles, and use the quartering method to reduce them to about 1 / 4 of the mass, and test to obtain the second particle strength coefficient; 3. When the difference between the strength coefficient of the second particle and the strength coefficient of the first particle is 3%-4%, the needle coke particles obtained are used for the subsequent production of carbon products or graphite.
2. The method for testing the strength of needle coke particles according to claim 1, wherein: 1 kg of the needle coke is selected and reduced by quartering to a mass of 250 g having a purity of not less than 95%.