Method for measuring content of iron element in ternary positive electrode material
Through two digestion treatments and the coordination reaction of ICP-OES combined with aqueous ammonia solution, cobalt and iron were separated, and the problem of insufficient accuracy in determining iron content in ternary positive electrode materials was solved, achieving high accuracy and high stability Determination results.
Patent Information
- Application Number
- CN202410960416.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, when measuring impurity elements in ternary positive electrode materials, complex matrix interference, element spectral lines overlap and pretreatment errors lead to insufficient measurement accuracy and stability, especially the iron content is difficult to accurately determine.
Two digestion treatments and inductively coupled plasma emission spectrometer (ICP-OES) combined with the coordination reaction of aqueous ammonia solution were used to separate cobalt and iron, and the iron content was quantitatively determined by standard curve method.
The accuracy and stability of iron content measurement were improved, and the recovery rate of the measurement results was as high as 110%, and the relative standard deviation was less than 4.12%, proving the high accuracy and good precision of the method.
Smart Images

Figure CN118914170A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of testing the content of impurity elements in positive electrode materials, and specifically relates to a method for measuring the content of iron elements in a ternary positive electrode material. Background Art
[0002] Ternary cathode materials have become one of the hot spots in the current research and application of lithium-ion batteries due to their advantages of high energy density, high voltage platform and good cycle stability. They are widely used in portable electronic devices, electric vehicles and large-scale energy storage systems. Ternary cathode materials refer to composite oxide materials composed of three different transition metal elements (usually nickel, cobalt, manganese) and lithium and oxygen. The chemical formula of this cathode material is usually expressed as LiNi x Co y Mn z O2, where the values of x, y, and z determine the content of different transition metal elements, thereby affecting the electrochemical properties and safety performance of the positive electrode material. Specifically, increasing the content of nickel can increase the energy density of the ternary positive electrode material, increasing the content of cobalt can improve the cycle stability of the ternary positive electrode material, and increasing the content of manganese can improve the structural stability of the ternary positive electrode material. However, during the processing and synthesis of the ternary positive electrode material, impurity elements (such as iron) may be introduced, resulting in a decrease in the cycle stability, energy storage performance, and safety performance of the lithium-ion battery. Therefore, in order to ensure the electrochemical performance and safety of lithium-ion batteries, it is of great significance to be able to accurately determine the impurity elements in the ternary positive electrode material.
[0003] At present, the determination of impurity elements in ternary positive electrode materials may face the following problems: First, the complex matrix of the ternary positive electrode material may interfere with the determination of metal impurity elements and affect the accuracy of the analysis results; second, when performing spectral analysis, the spectral lines of different elements may overlap, making it difficult to accurately determine the content of specific metal impurity elements. For example, since the wavelength spectrum of the cobalt element is 238.176nm, which is very close to the wavelength spectrum of the iron element (238.204nm), the main cobalt element in the ternary positive electrode material affects the determination of the impurity iron element content; finally, the metal impurity elements in the ternary positive electrode material usually require specific pre-treatment steps to be accurately determined, and this step may introduce errors or contamination. For example, the ordinary wet digestion method disclosed in the prior art cannot completely digest the carbon-based material or digests it with difficulty, and it is impossible to determine whether the digestion is complete, and the repeatability of the treatment process is poor.
[0004] Therefore, in this field, there is an urgent need to develop a method for accurately determining the impurity elements in the ternary positive electrode material to solve the above-mentioned problem. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for determining the iron content in a ternary positive electrode material, thereby improving the accuracy and stability of the determination.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for determining the iron content in a ternary positive electrode material, the method comprising the following steps:
[0008] The sample to be tested is subjected to a first digestion treatment to obtain a solution containing iron ions; the solution containing iron ions is subjected to a precipitation reaction to obtain an insoluble substance containing iron elements;
[0009] The insoluble matter containing the iron element is subjected to a second digestion treatment to obtain a test solution; and the iron element content in the test solution is determined by an inductively coupled plasma emission spectrometer.
[0010] The present invention digests the sample to be tested, obtains the precipitated insoluble matter containing the iron element by using an ammonia solution, and then digests the insoluble matter containing the iron element, and uses an inductively coupled plasma optical emission spectrometer (ICP-OES) to determine the iron element in the ternary positive electrode material. This is mainly due to the coordination reaction between the trivalent cobalt ions in the ternary positive electrode material and the ammonia solution. The reaction formula is as follows: in the coordination reaction, the trivalent cobalt ions (Co(H2O)6 3+ ) is replaced by six ammonia molecules to form the hexaamminecobalt(III) ion ([Co(NH3)6] + ), and the coordination compound formed is soluble in water, so as to separate the cobalt element and the iron element, thereby eliminating the influence of the cobalt element on the iron element test.
[0011]
[0012] Preferably, the sample to be tested includes a nickel-cobalt-lithium manganese oxide ternary positive electrode material.
[0013] Preferably, the chemical formula of the nickel-cobalt-manganese-lithium ternary positive electrode material is LiNi x Co y Mn 1-x-y O2, where the value range of x is 0<x<1, and the value range of y is 0<y<1.
[0014] Preferably, the first digestion treatment process includes heating the sample to be tested and hydrochloric acid for the first time.
[0015] Preferably, the mass of the sample to be tested is 0.5g-2g, for example, it can be 0.5g, 0.8g, 1g, 1.2g, 1.5g, 1.8g, 2g, etc.
[0016] Preferably, the volume of the hydrochloric acid is 5 mL-20 mL, for example, 5 mL, 6 mL, 8 mL, 10 mL, 12 mL, 15 mL, 18 mL, or 20 mL.
[0017] In the present invention, the sample can be completely dissolved by adjusting the mass of the sample to be tested and the volume of hydrochloric acid.
[0018] Preferably, the temperature of the first heating treatment is 100-200°C, for example, 100°C, 120°C, 150°C, 180°C, 200°C, etc.
[0019] Preferably, the precipitation reaction process includes subjecting the solution containing iron ions to a precipitation reaction with a weak alkaline solution to obtain an insoluble substance containing iron elements.
[0020] Preferably, the weak alkaline solution comprises an aqueous ammonia solution.
[0021] Preferably, the volume of the weak base solution is 20 mL.
[0022] In the present invention, the iron ions are completely precipitated by regulating the content relationship between the solution containing iron ions and the weak alkaline solution.
[0023] Preferably, the precipitation reaction is carried out under ultrasound.
[0024] Preferably, the ultrasonication time is 1 h.
[0025] Preferably, the precipitation reaction further includes centrifugation and washing.
[0026] Preferably, the washing treatment is performed using aqueous ammonia.
[0027] In the present invention, the process of washing with ammonia water includes washing with ammonia water three times.
[0028] Preferably, the second digestion treatment process includes subjecting the insoluble matter containing iron elements and hydrochloric acid to a second heating treatment.
[0029] Preferably, the volume of the hydrochloric acid is 10 mL.
[0030] Preferably, the temperature of the second heating treatment is 150°C.
[0031] Preferably, the second digestion process further includes a volume fixing process.
[0032] In the present invention, after the second digestion treatment is completed, the product is cooled and then subjected to constant volume treatment.
[0033] Preferably, the volume is fixed to 10 mL.
[0034] In the present invention, the volume fixing treatment includes adding ultrapure water to a volume of 10 mL.
[0035] Preferably, the working gas in the inductively coupled plasma optical emission spectrometer is argon with a purity of 99.999%.
[0036] Preferably, the instrument detection conditions of the inductively coupled plasma emission spectrometer include: plasma RF power of 1200W; plasma gas flow rate of 12L / min; auxiliary gas flow rate of 1L / min; nebulizer gas flow rate of 0.7L / min; peristaltic pump speed of 12rpm; and iron element wavelength spectrum line of 238.204nm.
[0037] Preferably, the iron content in the test liquid is measured by an inductively coupled plasma emission spectrometer, and a standard curve method is used for quantitative determination to obtain iron content data; wherein the standard curve method comprises the following steps:
[0038] S1. Pipette the standard solution of iron element and dilute it with ultrapure water in a volumetric flask that has passed the measurement and calibration to obtain a series of standard curve solutions with different concentration gradients;
[0039] S2. The standard curve solution in step S1 is analyzed using an inductively coupled plasma emission spectrometer to obtain a linear relationship between the wavelength spectral line intensity and mass concentration of iron at 238.204 nm. The equipment automatically draws a working curve of the standard curve solution and gives a regression equation and correlation coefficient of the working curve.
[0040] S3. Analyze the test liquid and obtain the spectral line intensity of the iron element in the test liquid at a wavelength of 238.204nm. The equipment will calculate the iron content data based on the regression equation of the working curve in step S2 and the known mass concentration of the iron element in the standard curve solution.
[0041] Preferably, the regression equation of the working curve is: y=3013.06579046×x+13.07798676, and the correlation coefficient is 0.99999.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] The present invention provides a method for determining the content of iron in a ternary positive electrode material, wherein the method comprises the following steps: digesting a sample to be tested, obtaining a precipitated insoluble matter containing iron using an ammonia solution, then digesting the insoluble matter containing iron, and using an inductively coupled plasma optical emission spectrometer (ICP-OES) to determine the iron in the ternary positive electrode material. This is mainly due to the fact that a coordination reaction will occur between the trivalent cobalt ions in the ternary positive electrode material and the ammonia solution. The reaction formula is as follows: in the coordination reaction, the trivalent cobalt ions (Co(H2O)6 3+ ) is replaced by six ammonia molecules to form the hexaamminecobalt(III) ion ([Co(NH3)6] + ), and the coordination compound formed is soluble in water, so as to separate the cobalt element and the iron element, thereby eliminating the influence of the cobalt element on the iron element test.
[0044] The method for determining the content of iron in the ternary positive electrode material provided by the present invention performs a spike recovery experiment on a nickel cobalt manganese oxide lithium sample under the same ICP-OES optimization conditions. The recovery rate of iron measured by the method is as high as 110%, which proves that the method has high accuracy. In addition, the present invention also performs precision analysis on the detection results in parallel samples of nickel cobalt manganese oxide lithium, and the minimum relative standard deviation is 4.12%, which proves that the method has good precision. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is the spectrum of iron element measured in Example 1 of the present invention;
[0046] Figure 2 This is the spectrum of iron element measured in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below by combining the accompanying drawings and specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0048] Example 1
[0049] This embodiment provides a method for determining the iron content in a nickel-cobalt-lithium manganese oxide ternary positive electrode material, the method comprising the following steps:
[0050] 0.5g of sample 1 was placed in a polytetrafluoroethylene beaker, and 5mL of hydrochloric acid was added. The solution was heated at 150°C for the first digestion treatment until the sample 1 was completely dissolved, and then the solution was evaporated. After cooling, a small amount of ultrapure water was added to obtain a solution containing iron ions; the solution containing iron ions and 30mL of ammonia water were subjected to precipitation reaction under ultrasound. After ultrasound for 1h, the precipitate was separated by centrifugation, and the precipitate was washed three times with 20mL of ammonia water, and the insoluble matter containing iron was obtained after centrifugation;
[0051] The insoluble matter containing iron and 10 mL of hydrochloric acid are digested for the second time at 150° C. until the solution is the size of soybean grains, cooled, and fixed to a volume of 10 mL to obtain a test solution; the iron content in the test solution is determined by an inductively coupled plasma emission spectrometer, and the standard curve method is used for quantitative determination to obtain the iron content data; wherein the standard curve method includes the following steps:
[0052] S1. Pipette the standard solution of iron element and dilute it with ultrapure water in a volumetric flask that has passed the measurement and calibration to obtain a series of standard curve solutions with different concentration gradients;
[0053] S2. The standard curve solution in step S1 is analyzed using an inductively coupled plasma emission spectrometer to obtain a linear relationship between the wavelength spectral intensity and mass concentration of the iron element at 238.204 nm. The equipment automatically draws a working curve of the standard curve solution and gives a regression equation and correlation coefficient of the working curve. Specifically, the regression equation of the working curve is: y=3013.06579046×x+13.07798676, and the correlation coefficient is 0.99999;
[0054] S3. Analyze the test liquid and obtain the spectral line intensity of the iron element in the test liquid at a wavelength of 238.204nm. The equipment will calculate the iron content data based on the regression equation of the working curve in step S2 and the known mass concentration of the iron element in the standard curve solution.
[0055] The instrument detection conditions of the inductively coupled plasma emission spectrometer in this embodiment include: the plasma RF power is 1200W; the working gas is high-purity argon with a purity of 99.999%; the plasma gas flow rate is 12L / min; the auxiliary gas flow rate is 1L / min; the nebulizer gas flow rate is 0.7L / min; the peristaltic pump speed is 12rpm; and the wavelength spectrum of the iron element is 238.204nm.
[0056] Example 2
[0057] This embodiment provides a method for determining the iron content in a nickel-cobalt-lithium manganese oxide ternary positive electrode material, the method comprising the following steps:
[0058] Place 1g of sample 2 in a polytetrafluoroethylene beaker, add 5mL of hydrochloric acid, and heat at 150°C for the first digestion treatment. After sample 2 is completely dissolved, evaporate the solution. After cooling, add a small amount of ultrapure water to obtain a solution containing iron ions; the solution containing iron ions and 20mL of ammonia water are subjected to precipitation reaction under ultrasound. After ultrasound for 1h, the precipitate is separated by centrifugation, and the precipitate is washed three times with 10mL of ammonia water. After centrifugation, the insoluble matter containing iron elements is obtained;
[0059] The insoluble matter containing iron and 10 mL of hydrochloric acid are digested for the second time at 150° C. until the solution is the size of soybean grains, cooled, and fixed to a volume of 10 mL to obtain a test solution; the iron content in the test solution is determined by an inductively coupled plasma emission spectrometer, and the standard curve method is used for quantitative determination to obtain the iron content data; wherein the standard curve method includes the following steps:
[0060] S1. Pipette the standard solution of iron element and dilute it with ultrapure water in a volumetric flask that has passed the measurement and calibration to obtain a series of standard curve solutions with different concentration gradients;
[0061] S2. The standard curve solution in step S1 is analyzed using an inductively coupled plasma emission spectrometer to obtain a linear relationship between the wavelength spectral intensity and mass concentration of the iron element at 238.204 nm. The equipment automatically draws a working curve of the standard curve solution and gives a regression equation and correlation coefficient of the working curve. Specifically, the regression equation of the working curve is: y=3013.06579046×x+13.07798676, and the correlation coefficient is 0.99999;
[0062] S3. Analyze the test liquid and obtain the spectral line intensity of the iron element in the test liquid at a wavelength of 238.204nm. The equipment will calculate the iron content data based on the regression equation of the working curve in step S2 and the known mass concentration of the iron element in the standard curve solution.
[0063] The instrument detection conditions of the inductively coupled plasma emission spectrometer in this embodiment include: the plasma RF power is 1200W; the working gas is high-purity argon with a purity of 99.999%; the plasma gas flow rate is 12L / min; the auxiliary gas flow rate is 1L / min; the nebulizer gas flow rate is 0.7L / min; the peristaltic pump speed is 12rpm; and the wavelength spectrum of the iron element is 238.204nm.
[0064] Comparative Example 1
[0065] This comparative example provides a method for determining the iron content in a nickel-cobalt-lithium-manganese oxide ternary positive electrode material, the method comprising the following steps:
[0066] 1 g of sample 2 is placed in a polytetrafluoroethylene beaker, and 5 mL of hydrochloric acid is added, and the solution is heated at 150° C. for digestion treatment. After the sample 2 is completely dissolved, the solution is further heated until it becomes the size of a soybean grain, cooled, and fixed to a volume of 10 mL to obtain a test solution; the iron content in the test solution is determined by an inductively coupled plasma emission spectrometer, and the standard curve method is used for quantitative determination to obtain the iron content data; wherein the standard curve method comprises the following steps:
[0067] S1. Pipette the standard solution of iron element and dilute it with ultrapure water in a volumetric flask that has passed the measurement and calibration to obtain a series of standard curve solutions with different concentration gradients;
[0068] S2. The standard curve solution in step S1 is analyzed using an inductively coupled plasma emission spectrometer to obtain a linear relationship between the wavelength spectral intensity and mass concentration of the iron element at 238.204 nm. The equipment automatically draws a working curve of the standard curve solution and gives a regression equation and correlation coefficient of the working curve. Specifically, the regression equation of the working curve is: y=3013.06579046×x+13.07798676, and the correlation coefficient is 0.99999;
[0069] S3. Analyze the test liquid and obtain the spectral line intensity of the iron element in the test liquid at a wavelength of 238.204nm. The equipment will calculate the iron content data based on the regression equation of the working curve in step S2 and the known mass concentration of the iron element in the standard curve solution.
[0070] The instrument detection conditions of the inductively coupled plasma emission spectrometer in this embodiment include: the plasma RF power is 1200W; the working gas is high-purity argon with a purity of 99.999%; the plasma gas flow rate is 12L / min; the auxiliary gas flow rate is 1L / min; the nebulizer gas flow rate is 0.7L / min; the peristaltic pump speed is 12rpm; and the wavelength spectrum of the iron element is 238.204nm.
[0071] Test Examples 1-2 and Comparative Test Example 1
[0072] This test example evaluates the precision and accuracy of the measurement methods of Examples 1-2 and Comparative Example 1.
[0073] (1) Precision test
[0074] Two samples of positive electrode materials of the battery were taken in parallel for each of Examples 1-2 and Comparative Example 1, and the experiments were carried out in parallel. The results were calculated based on the content of iron element. The precision test results are shown in Table 1:
[0075] Table 1
[0076]
[0077] It can be seen from Table 1 that when the parallel sample test is carried out using the method provided by the present invention, the relative standard deviation RSD is no higher than 12%, and the relative standard deviation meets the requirements of element analysis.
[0078] (2) Accuracy test
[0079] The test solutions of Examples 1-2 and Comparative Example 1 were subjected to sample spike recovery tests. The results are shown in Table 2:
[0080] Table 2
[0081]
[0082] From the results of the spike recovery test in Table 2, it can be seen that the recovery rate of the standard product obtained is between 95% and 96%, which meets the requirements for element detection. Figure 1-Figure 2 The relative peak height in the emission spectrum is higher than that of the iron element obtained by ordinary wet digestion test, and the relative peak is more obvious, so the test data obtained is more accurate.
[0083] In summary, the method for determining the iron content in the ternary positive electrode material provided by the present invention has good accuracy and reproducibility.
[0084] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for determining the iron content in a ternary positive electrode material, characterized in that: The method comprises the following steps: The sample to be tested is subjected to a first digestion treatment to obtain a solution containing iron ions; the solution containing iron ions is subjected to a precipitation reaction to obtain an insoluble substance containing iron elements; The insoluble matter containing the iron element is subjected to a second digestion treatment to obtain a test solution; and the iron element content in the test solution is determined by an inductively coupled plasma emission spectrometer.
2. The method according to claim 1, characterized in that The sample to be tested includes a nickel-cobalt-lithium manganese oxide ternary positive electrode material; Preferably, the chemical formula of the nickel-cobalt-manganese-lithium ternary positive electrode material is LiNi x Co y Mn 1-x-y O2, where the value range of x is 0<x<1, and the value range of y is 0<y<1.
3. The method according to claim 1 or 2, characterized in that: The first digestion process includes heating the sample to be tested and hydrochloric acid for the first time; Preferably, the mass of the sample to be tested is 0.5g-2g; Preferably, the volume of the hydrochloric acid is 5mL-20mL; Preferably, the temperature of the first heating treatment is 100-200°C.
4. The method according to any one of claims 1 to 3, characterized in that The precipitation reaction process includes subjecting the solution containing iron ions to a precipitation reaction with a weak base solution to obtain an insoluble substance containing iron elements; Preferably, the weak alkaline solution comprises an aqueous ammonia solution; Preferably, the volume of the weak base solution is 20 mL; Preferably, the precipitation reaction is carried out under ultrasound; Preferably, the ultrasonic time is 1h; Preferably, after the precipitation reaction is completed, centrifugation and washing are also included; Preferably, the washing treatment is performed using aqueous ammonia.
5. The method according to any one of claims 1 to 4, characterized in that The second digestion process includes heating the insoluble matter containing iron and hydrochloric acid for a second time; Preferably, the volume of the hydrochloric acid is 10 mL; Preferably, the temperature of the second heating treatment is 150°C.
6. The method according to any one of claims 1 to 5, characterized in that After the second digestion process is completed, a constant volume process is also included; Preferably, the volume is fixed to 10 mL.
7. The method according to any one of claims 1 to 6, characterized in that The working gas in the inductively coupled plasma emission spectrometer is argon gas with a purity of 99.999%.
8. The method according to any one of claims 1 to 7, characterized in that The instrument detection conditions of the inductively coupled plasma emission spectrometer include: plasma radio frequency power of 1200W; plasma gas flow rate of 12L / min; auxiliary gas flow rate of 1L / min; nebulizer gas flow rate of 0.7L / min; peristaltic pump speed of 12rpm; and iron element wavelength spectrum line of 238.204nm.
9. The method according to any one of claims 1 to 8, characterized in that The iron content in the test liquid is measured by inductively coupled plasma emission spectrometer, and the standard curve method is used for quantitative determination to obtain the iron content data; wherein the standard curve method comprises the following steps: S1. Pipette the standard solution of iron element and dilute it with ultrapure water in a volumetric flask that has passed the measurement and calibration to obtain a series of standard curve solutions with different concentration gradients; S2. The standard curve solution in step S1 is analyzed using an inductively coupled plasma emission spectrometer to obtain a linear relationship between the wavelength spectral line intensity and mass concentration of iron at 238.204 nm. The equipment automatically draws a working curve of the standard curve solution and gives a regression equation and correlation coefficient of the working curve. S3. Analyze the test liquid and obtain the spectral line intensity of the iron element in the test liquid at a wavelength of 238.204nm. The equipment will calculate the iron content data based on the regression equation of the working curve in step S2 and the known mass concentration of the iron element in the standard curve solution.
10. The method according to any one of claims 1 to 9, characterized in that The regression equation of the working curve is: y=3013.06579046×x+13.07798676, and the correlation coefficient is 0.99999.