Multi-stage infrared laser modulation structure based on vanadium dioxide film and preparation method of multi-stage infrared laser modulation structure
By stacking a multi-layer structure on a sapphire substrate, including the first, vanadium dioxide film layer and a vanadium dioxide film layer doped with tungsten element, combined with the PMMA protective layer, the modulation of a single vanadium dioxide film in laser protection is solved. The problem of poor effect and easy oxidation achieves multi-stage infrared laser modulation and long-term stability.
Patent Information
- Application Number
- CN202410799821.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-20
AI Technical Summary
The single-layer vanadium dioxide film has poor modulation effect in laser protection and is prone to oxidation failure, which cannot effectively prevent the damage of the blinding laser to the photodetection equipment.
A multi-stage infrared laser modulated vanadium dioxide film structure was designed, and the excitation phase was reduced by stacking the first, vanadium dioxide film layer, tungsten-doped vanadium dioxide film layer and PMMA protective layer on a sapphire substrate. Change the laser power threshold, improve the modulation effect, and add a protective layer to prevent oxidation.
The multi-stage modulation effect at different laser powers is achieved, the laser power threshold is reduced, the protection performance of laser light is improved, and it does not fail in long-term use in air, which is low in cost and non-toxic.
Smart Images

Figure CN118915336A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laser protection, and in particular to a vanadium dioxide thin film junction with multi-level infrared laser modulation and a preparation method thereof. Background Art
[0002] Electro-detection equipment is one of the important sensing devices of integrated avionics systems. Many types of aircraft at home and abroad are equipped with advanced tracking and targeting pods or airborne infrared search and tracking (IRST) systems, electro-optical surveillance and reconnaissance and other electro-optical equipment. However, without protection, electro-optical detection equipment is extremely vulnerable to damage from modern blinding laser weapons, resulting in functional failure. Blinding lasers can destroy the structural materials, optical devices and sensor films of electro-optical equipment, damage the entire component and system, and even raise the temperature of the opto-electronic equipment cabin or key components to the melting point and ablate or reach the failure temperature of the structure, thereby threatening the survivability of the carrier aircraft.
[0003] VO2 will undergo phase change under certain external stimuli (including laser, heat, electric field, etc.), changing from high infrared transmittance to low transmittance. When normal low-energy signal light enters the detection device, the VO2 film can maintain high transmittance to ensure normal signal transmission; when a strong blinding laser strikes, a phase change occurs, reducing transmittance to prevent damage to internal components. At the same time, VO2 has a low phase change threshold and can undergo phase change within femtoseconds. Both continuous lasers and pulsed lasers can cause its phase change, which can provide effective protection and is considered to be an excellent laser protection material.
[0004] Selecting different ion doping has different effects on vanadium dioxide, including crystal structure, grain size, etc., which will have a direct impact on the film's phase transition temperature, resistivity, thermal hysteresis loop width, transmittance and reflectivity. Therefore, selecting appropriate elements to dope VO2 thin film is important for further understanding the phase transition principle of vanadium dioxide and expanding its practical application. Among the many doping elements, the addition of tungsten has a significant effect on reducing the phase transition temperature of VO2 thin film.
[0005] However, the infrared transmittance of a single layer of vanadium dioxide is high, and the absorption rate is low. When the laser power is low, it is not easy to excite the phase change, the response time is slow, and the modulation effect is poor. In addition, vanadium dioxide is easily oxidized to vanadium pentoxide and becomes ineffective when exposed to air for a long time. Therefore, the optical structure of vanadium dioxide film is of great significance for its application in laser protection. Summary of the invention
[0006] In view of the problem that the single-layer vanadium dioxide has poor modulation effect and is easily oxidized and becomes ineffective in the background technology, the purpose of the present invention is to provide a vanadium dioxide thin film structure with multi-level infrared laser modulation and a preparation method thereof. The present invention designs a vanadium dioxide thin film structure with multi-level infrared laser modulation, reduces the laser power threshold for exciting the phase change of vanadium dioxide, improves the modulation effect of the laser, and exhibits a multi-level modulation effect under different laser powers.
[0007] To achieve the above-mentioned purpose, the technical scheme of the present invention is as follows: a multi-level infrared laser modulation structure based on vanadium dioxide thin film, which is stacked in sequence from bottom to top: a first vanadium dioxide thin film layer, a sapphire substrate, a second vanadium dioxide thin film layer, a tungsten-doped vanadium dioxide thin film layer, and a PMMA layer; the PMMA layer is a protective layer; the tungsten-doped vanadium dioxide thin film layer is an absorption layer; the first vanadium dioxide thin film layer and the second vanadium dioxide thin film layer are phase change functional layers.
[0008] Furthermore, the thickness of the first vanadium dioxide thin film layer and the second vanadium dioxide thin film layer is 100-200 nm.
[0009] Furthermore, the thickness of the PMMA layer is 300-500 nm; the thickness of the sapphire substrate is 0.5 mm.
[0010] Furthermore, the thickness of the vanadium dioxide thin film layer doped with tungsten element is 30 nm.
[0011] Furthermore, the tungsten doping concentration of the tungsten-doped vanadium dioxide thin film layer is 0.3-0.5 atomic percent.
[0012] A method for preparing a multi-level infrared laser modulation structure based on a vanadium dioxide film, the method comprising:
[0013] Step 1: preparing a precursor solution containing vanadium ions and a precursor solution doped with tungsten elements;
[0014] The specific method for preparing the precursor solution containing vanadium ions is as follows: weigh ammonium metavanadate and polyethyleneimine in a molar ratio of 1:1, add them to deionized water, and stir until the drugs are completely dissolved; finally, transfer the solution to an ultrafiltration device, add 0.2 atmospheres of pressure during filtration and perform magnetic stirring to remove water from the solution; during the preparation process, the pressurized ultrafiltration needs to be repeated more than three times, and the same amount of deionized water needs to be added each time until the last ultrafiltration is completed; a gas with a stable property needs to be introduced during the pressurized ultrafiltration process; the purpose of the pressurized ultrafiltration is to remove the small molecules remaining in the solution, further improve the stability of the precursor solution, and finally obtain a vanadium ion precursor solution with a concentration of 0.471 mmol / mL;
[0015] Step 2: Double-sided polishing and cleaning of the sapphire substrate and drying with nitrogen;
[0016] Step 3: Spin-coating a precursor solution containing vanadium ions on one side of the sapphire substrate, and sintering the solution in a mixed atmosphere of nitrogen and water vapor to prepare a vanadium dioxide thin film layer;
[0017] Step 4: Prepare a vanadium dioxide thin film layer on the other side of the sapphire substrate using the same method as step 3;
[0018] Step 5: Spin-coating a tungsten-doped precursor solution on the vanadium dioxide thin film layer on one side, and sintering the vanadium dioxide thin film layer in a mixed atmosphere of nitrogen and water vapor to obtain a tungsten-doped vanadium dioxide thin film layer;
[0019] Step 6: Spin-coat a PMMA solution on the tungsten-doped vanadium dioxide thin film layer and then cure it.
[0020] Furthermore, the concentration of tungsten in the tungsten-doped precursor solution is 0.3%-0.5% atomic concentration.
[0021] Furthermore, the substrate is double-polished sapphire with an orientation of (10-10), and the specific cleaning process is: ultrasonic cleaning with acetone, anhydrous ethanol and deionized water respectively.
[0022] Further, the sintering method in step 3 is:
[0023] First, the temperature was raised to 100°C and maintained for 30 minutes to remove moisture from the precursor solution; then the temperature was raised to 450°C and maintained for 240 minutes to remove the glue, and then the temperature was raised to 495°C and maintained for 240 minutes to form nuclei. After the reaction was completed, the temperature was naturally lowered to room temperature.
[0024] Furthermore, the specific parameters of the spin coating method in step 3 and step 6 are: first rotating at a relatively low speed of 900-1000 r / min for 10 s, and then rotating at a relatively high speed of 6000-7000 r / min for 40 s.
[0025] Furthermore, the specific parameters of curing in step 6 are: temperature of 180-200° C. and time of 40-60 min.
[0026] Furthermore, the wavelength of the modulated infrared laser is 1550 nm, and the power is 0-1100 mW.
[0027] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0028] The present invention designs a vanadium dioxide thin film structure with multi-level infrared laser modulation. By reasonably regulating the thin film structure, an absorption layer is added to reduce the laser power threshold for exciting the phase change of vanadium dioxide. The phase change functional layer improves the modulation effect on the laser and exhibits a multi-level modulation effect under different laser powers. The protective layer allows the sample to serve for a long time in the air and is suitable for a variety of applications. The prepared thin film is epitaxially grown, has excellent photoelectric properties, and the entire preparation method is low-cost and non-toxic. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the structure of the vanadium dioxide film of the present invention.
[0030] Figure 2 This is a near-infrared transmission spectrum of the vanadium dioxide film prepared in Example 1.
[0031] Figure 3 This is the near-infrared transmission spectrum of the vanadium dioxide film prepared in Comparative Example 1.
[0032] Figure 4 This is the 1550nm infrared laser modulation diagram of the vanadium dioxide film prepared in Example 1.
[0033] Figure 5 This is the 1550nm infrared laser modulation diagram of the vanadium dioxide film prepared in Comparative Example 1. DETAILED DESCRIPTION
[0034] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the implementation modes and the accompanying drawings.
[0035] A vanadium dioxide thin film structure with multi-level infrared laser modulation includes a phase change layer arranged on both sides of a substrate and a protective layer arranged on the phase change layer. The phase change layer is composed of an absorption layer and a phase change functional layer, the absorption layer is a tungsten-doped vanadium dioxide thin film, the phase change functional layer is a high-quality vanadium dioxide thin film, and the protective layer is a material with high infrared transmittance.
[0036] The method for preparing the vanadium dioxide film comprises the following steps:
[0037] A polymer precursor solution containing vanadium ions and a precursor solution doped with tungsten were prepared by polymer-assisted deposition method, and a vanadium dioxide thin film phase change functional layer was grown on both sides of the cleaned double-polished sapphire substrate. Then, a tungsten-doped vanadium dioxide thin film absorption layer was deposited on the sample with the vanadium dioxide thin film grown. Finally, a layer of PMMA was spin-coated on the surface of the absorption layer, and the cured PMMA was used as a protective layer.
[0038] Example 1
[0039] The method for preparing the vanadium dioxide film comprises the following steps:
[0040] Step 1: Prepare a vanadium ion precursor solution and a tungsten-doped precursor solution according to the polymer assisted deposition method; the specific method for preparing the vanadium ion precursor solution is: weigh ammonium metavanadate and polyethyleneimine with a molar ratio of 1:1, add them to deionized water, and stir until the drug is completely dissolved; finally, transfer the solution to an ultrafiltration device, add 0.2 atmospheres of pressure during filtration and perform magnetic stirring to remove water from the solution; during the preparation process, pressurized ultrafiltration needs to be repeated more than three times, and the same amount of deionized water needs to be added each time until the last ultrafiltration is completed; during the pressurized ultrafiltration process, a gas with stable properties needs to be introduced: argon or nitrogen; the purpose of pressurized ultrafiltration is to remove small molecules remaining in the solution, further improve the stability of the precursor solution, and finally obtain a vanadium ion precursor solution with a concentration of 0.471mmol / mL;
[0041] Step 2: Clean the Al2O3 substrate by ultrasonic cleaning it with acetone, anhydrous ethanol and deionized water in sequence, and then blow dry it with nitrogen for later use;
[0042] Step 3: Spin-coat the vanadium ion precursor solution prepared in step 1 onto one side of the cleaned sapphire substrate by spin coating, first at a low speed of 1000 r / min for 10 seconds, and then at a high speed of 6000 r / min for 40 seconds;
[0043] Step 4: Install the heat-insulating furnace plug at the air inlet of the tube furnace, place the substrate on which the precursor solution is spin-coated in step 3 on an inverted quartz porcelain boat and put it in the center of the tube furnace, seal it with a flange, place the gas duct in a beaker filled with water, and sinter in a mixed atmosphere of nitrogen and water vapor, and observe the bubbling in the beaker to detect the sealing effect; start the set tube furnace program: heat up to 100°C and keep it for 30 minutes to remove moisture from the precursor solution, heat up to 450°C and keep it for 240 minutes to remove the glue, then heat up to 495°C and keep it for 240 minutes to form nuclei, and naturally cool it to room temperature after the reaction is completed to obtain a VO2 / Al2O3 sample;
[0044] Step 5: Repeat the above steps to deposit VO2 on the other side of Al2O3 to obtain VO2 / Al2O3 / VO2 sample;
[0045] Step 6: Spin-coat the tungsten-doped precursor solution prepared in step 1 onto the sample prepared in step 5 by spin coating, perform spin coating according to the parameters of step 3, and repeat step 4 to obtain a W-VO2 / VO2 / Al2O3 / VO2 sample;
[0046] Step 7: Spin-coat the PMMA solution on the sample prepared in step 6, keep it at a low speed of 1000 r / min for 10 seconds, and then keep it at a high speed of 6000 r / min for 40 seconds, and place the sample on a 180°C hot stage for curing for 30 minutes to obtain a PMMA / W-VO2 / VO2 / Al2O3 / VO2 sample;
[0047] The near infrared transmission spectrum of the vanadium dioxide film prepared in this example is shown in Figure 2 As shown, the blue line represents the near-infrared transmittance curve of the sample before phase change (30°C), and the red line represents the near-infrared transmittance curve of the sample after phase change (90°C). The specific expression of infrared modulation depth is as follows:
[0048]
[0049] Where M is the modulation depth of the sample, T1 is the transmittance of the sample before the phase change (30°C), and T2 is the transmittance of the sample after the phase change (90°C).
[0050] The transmittance of the sample at 1550nm is 40.07% before phase change, 4.88% after phase change, and the modulation depth of the sample at 1550nm is 87.82%. The transmittance of the sample at 2500nm is 59.06% before phase change, 2.74% after phase change, and the modulation depth of the sample at 2500nm is 95.37%.
[0051] Figure 4 This is the modulation diagram of the 1550nm continuous laser of the sample. When the laser power is low, the sample will not undergo phase change. The power is increased by 100mW every 20s and maintained for 20s. The power waveform is observed to determine whether the sample has phase change. When the laser power rises to 800mW, the sample undergoes obvious phase change. At this time, the power is increased by 50mW every 20s and maintained for 20s. Analysis Figure 4 It can be seen that the sample undergoes a phase change after 18.7s under a laser power of 700mW, and the modulation depth is 26.13% at this time. As the laser power increases further, the phase change time of the sample gradually becomes shorter, and different modulation effects are exhibited under different laser powers. When the laser power rises to 1000mW, the sample undergoes a phase change after 2.1s, and the modulation depth is 48.17%. When the laser power rises to 1100mW, the VO2 on the upper layer of the substrate undergoes a phase change after 0.1s, and the modulation depth is 48.88%. After 4.9s, the VO2 on the lower layer of the substrate undergoes a phase change, achieving secondary modulation, and the modulation depth reaches 75.24%.
[0052] Comparative Example 1
[0053] The VO2 / Al2O3 sample was prepared according to the steps in Example 1, and only steps 1 to 4 were repeated.
[0054] The transmittance of the sample at 1550nm is 63.11% before phase change, 33.07% after phase change, and the modulation depth of the sample at 1550nm is 47.60%. The transmittance of the sample at 2500nm is 80.56% before phase change, 22.05% after phase change, and the modulation depth of the sample at 2500nm is 72.63%.
[0055] Figure 4 The modulation diagram of the sample's 1550nm continuous laser is shown below. When the laser power is low, the sample will not undergo phase change. The power is increased by 100mW every 20s and maintained for 20s. The power waveform is observed to determine whether the sample undergoes phase change. When the laser power rises to 1000mW, the sample undergoes phase change after 9.3s, and the modulation depth is 36.83% at this time. When the laser power rises to 1100mW, the sample undergoes phase change after 3.4s, and the modulation depth is 45.30%.
[0056] The above description is only a specific implementation mode of the present invention. Any feature disclosed in this specification, unless otherwise stated, can be replaced by other alternative features that are equivalent or have similar purposes; all the disclosed features, or all the steps in the methods or processes, except for mutually exclusive features and / or steps, can be combined in any way.
Claims
1. A multi-level infrared laser modulation structure based on vanadium dioxide film, which is stacked from bottom to top in sequence: a first vanadium dioxide film layer, a sapphire substrate, a second vanadium dioxide film layer, a tungsten-doped vanadium dioxide film layer, and a PMMA layer; the PMMA layer is a protective layer; the tungsten-doped vanadium dioxide film layer is an absorption layer; the first vanadium dioxide film layer and the second vanadium dioxide film layer are phase change functional layers.
2. A multi-level infrared laser modulation structure based on vanadium dioxide thin film as claimed in claim 1, characterized in that: The thickness of the first vanadium dioxide thin film layer and the second vanadium dioxide thin film layer is 100-200 nm.
3. A multi-level infrared laser modulation structure based on vanadium dioxide thin film as claimed in claim 1, characterized in that: The thickness of the PMMA layer is 300-500 nm; the thickness of the sapphire substrate is 0.5 mm.
4. A multi-level infrared laser modulation structure based on vanadium dioxide thin film as claimed in claim 1, characterized in that: The thickness of the vanadium dioxide thin film layer doped with tungsten element is 30nm.
5. The multi-level infrared laser modulation structure based on vanadium dioxide film according to claim 1, characterized in that: The tungsten doping concentration of the tungsten-doped vanadium dioxide film layer is 0.3-0.5 atomic percent.
6. A method for preparing a multi-level infrared laser modulation structure based on vanadium dioxide film, the method comprising: Step 1: preparing a precursor solution containing vanadium ions and a precursor solution doped with tungsten elements; The specific method for preparing the precursor solution containing vanadium ions is as follows: weigh ammonium metavanadate and polyethyleneimine in a molar ratio of 1:1, add them to deionized water, and stir until the drugs are completely dissolved; finally, transfer the solution to an ultrafiltration device, add 0.2 atmospheres of pressure during filtration and perform magnetic stirring to remove water from the solution; during the preparation process, the pressurized ultrafiltration needs to be repeated more than three times, and the same amount of deionized water needs to be added each time until the last ultrafiltration is completed; a gas with a stable property needs to be introduced during the pressurized ultrafiltration process; the purpose of the pressurized ultrafiltration is to remove the small molecules remaining in the solution, further improve the stability of the precursor solution, and finally obtain a vanadium ion precursor solution with a concentration of 0.471 mmol / mL; Step 2: Double-sided polishing and cleaning of the sapphire substrate and drying with nitrogen; Step 3: Spin-coating a precursor solution containing vanadium ions on one side of the sapphire substrate, and sintering the solution in a mixed atmosphere of nitrogen and water vapor to prepare a vanadium dioxide thin film layer; Step 4: Prepare a vanadium dioxide thin film layer on the other side of the sapphire substrate using the same method as step 3; Step 5: Spin-coating a tungsten-doped precursor solution on the vanadium dioxide thin film layer on one side, and sintering the vanadium dioxide thin film layer in a mixed atmosphere of nitrogen and water vapor to obtain a tungsten-doped vanadium dioxide thin film layer; Step 6: Spin-coat a PMMA solution on the tungsten-doped vanadium dioxide thin film layer and then cure it.
7. The method for preparing a multi-level infrared laser modulation structure based on a vanadium dioxide thin film according to claim 6, characterized in that: The substrate is double-polished sapphire with an orientation of (10-10). The specific cleaning process is: ultrasonic cleaning with acetone, anhydrous ethanol and deionized water respectively.
8. The method for preparing a multi-level infrared laser modulation structure based on a vanadium dioxide thin film according to claim 6, characterized in that: The sintering method in step 3 is: First, the temperature was raised to 100°C and maintained for 30 minutes to remove moisture from the precursor solution; then the temperature was raised to 450°C and maintained for 240 minutes to remove the glue, and then the temperature was raised to 495°C and maintained for 240 minutes to form nuclei. After the reaction was completed, the temperature was naturally lowered to room temperature.
9. The method for preparing a multi-level infrared laser modulation structure based on a vanadium dioxide thin film according to claim 6, characterized in that: The specific parameters of the spin coating method in step 3 and step 6 are: firstly rotate at a relatively low speed of 900-1000 r / min for 10 s, and then rotate at a relatively high speed of 6000-7000 r / min for 40 s.
10. The method for preparing a multi-level infrared laser modulation structure based on a vanadium dioxide thin film according to claim 6, characterized in that: The specific parameters of curing in step 6 are: temperature of 180-200°C and time of 40-60 minutes.
Citation Information
Patent Citations
Preparation method of tungsten-doped vanadium dioxide film with adjustable phase change temperature
CN112921291A
Infrared radiation dynamic reconfigurable device and preparation method thereof
CN115200410A
Double-wave dynamic thermal camouflage structure and optimization method thereof
CN116088077A
A Tray for Planar Parts
KR1020210105532A
Solid state thermochromic device, and method for producing said device
US20190243036A1