Preparation method and application of capacitive deionization electrode for uranium solution enrichment

By preparing polydopamine-coated molybdenum disulfide material and mixing it with other materials, capacitive deionized electrodes for uranium solution enrichment are prepared, which solves the problem of low uranium enrichment efficiency of existing capacitive deionized electrodes and realizes uranium Efficient enrichment and regeneration of electrode materials.

CN118919117AInactive Publication Date: 2024-11-08EAST CHINA UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410797066.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing capacitive deionized electrodes have low uranium enrichment efficiency in uranium solution, the material is hydrophobic and lacks active sites, resulting in poor uranium enrichment efficiency.

Method used

By self-assembling the peeled molybdenum disulfide and dopamine hydrochloride in a buffer solution, adjusting the oscillation time to control the deposition amount of polydopamine, forming a polydopamine-coated molybdenum disulfide material, and mixing it with polyvinylidene fluoride and Kochen black, prepare Capacitive deionized electrodes for uranium solution enrichment are produced. The electrode material is prepared by sonication and vacuum freeze-drying, and finally coated on a titanium plate to assemble into a capacitive deionization system.

Benefits of technology

It significantly improves the uranium enrichment efficiency and saturation adsorption capacity in uranium solution. Compared with the original materials, the uranium enrichment capacity can be increased by 2 to 3 times, and the saturation adsorption capacity can be increased by 2 to 3 times, and the capacitor deionization system can be regenerated and cycled. Use 5 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919117A_ABST
    Figure CN118919117A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a capacitive deionization electrode for uranium solution enrichment, and relates to the preparation method and application of the capacitive deionization electrode. The technical problem that an existing capacitive deionization electrode is low in enrichment efficiency is solved. The preparation method comprises the following steps: 1, preparing MoS2 powder; (2) stripping MoS2; 3, adding polydopamine into the stripped MoS2 aqueous solution, oscillating and depositing, filtering, and drying to obtain a polydopamine coated molybdenum disulfide material; and 4, mixing the polydopamine-coated molybdenum disulfide material, polyvinylidene fluoride, ketjen black and N-methyl pyrrolidone to form slurry, coating a titanium substrate with the slurry, and drying to obtain the capacitive deionization electrode for uranium solution enrichment. When being used for enriching uranium in a uranium solution, the MoS2 can increase the uranium enrichment amount by 2-3 times and increase the saturation adsorption capacity by 2-3 times compared with MoS2. And after adsorption saturation, the electrode can be recycled for five times after regeneration. The electrode can be used in the field of uranium-containing wastewater treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a capacitor deionization electrode. Background Art

[0002] Uranium is an indispensable raw material for the development of the nuclear industry. Recovering uranium from uranium-containing solutions can not only reuse resources, but also reduce harm to the environment. The main methods for enriching uranium from uranium solutions include chemical precipitation, ion exchange, adsorption, photocatalysis and electrochemistry. Among them, the electrochemical method is simple, economical and universal. Capacitive deionization is one of them. It uses the electric field to adsorb the target ions on the surface of the electrode material, and achieves the enrichment of the target ions through physical adsorption, surface complexation, redox, ion exchange and / or electrostatic adsorption. The electrode material is the core of capacitive deionization, which is mainly composed of carbon materials, metal oxides and conductive polymers. For example, the composite material in the Chinese patent "A MoS2 / Porous Carbon Nanosphere Composite Material and Its Preparation Method" with application number CN201711476596.2 is a core-shell structure with porous nitrogen-doped carbon spheres as the core and molybdenum disulfide as the shell. The diameter of the composite sphere is between 500 and 600 nanometers. Molybdenum disulfide is evenly coated on the surface of the porous nitrogen-doped carbon spheres in a petal shape. However, when the material is used as a capacitive deionization electrode, the electrode has poor enrichment efficiency for uranium in uranium solution due to the hydrophobicity and lack of active sites. Summary of the invention

[0003] The present invention aims to solve the technical problem of low enrichment efficiency of the existing capacitor deionization electrode, and proposes a preparation method and application of a capacitor deionization electrode for enriching uranium solution.

[0004] The preparation method of the capacitor deionization electrode for uranium solution enrichment of the present invention comprises the following steps: self-assembling the stripped molybdenum disulfide and dopamine hydrochloride in a buffer solution, controlling the deposition amount of polydopamine by adjusting the oscillation time, obtaining the electrode material by vacuum freeze drying, and then coating the electrode material on a titanium plate to assemble the capacitor deionization electrode. The method is specifically carried out in the following steps:

[0005] 1. Preparation of MoS2 powder: (NH4)6Mo7O 24 The molar ratio of 4H2O to CN2H4S is 1:2. 24 4H2O and CN2H4S are added to deionized water, and after ultrasonic treatment, a uniform mixed solution is obtained; the mixed solution is then transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and hydrothermally treated at a temperature of 160-250°C for 6-8 hours; after the reaction is completed, it is naturally cooled to room temperature, and a black precipitate is collected by vacuum filtration with a microporous membrane, and then the precipitate is washed clean with deionized water, and then vacuum freeze-dried to obtain MoS2 powder;

[0006] 2. Add MoS2 powder to a Tris buffer solution with a pH of 7 to 10, and then put it into an ultrasonic cleaner, and ultrasonically treat it for 30 to 60 minutes at a power of 100 to 200 W and a frequency of 30 to 60 kHz to obtain an exfoliated MoS2 aqueous solution;

[0007] 3. Add polydopamine to the stripped MoS2 aqueous solution, shake at a speed of 180-200 rpm for 1-6 hours, filter, and freeze-dry the solid phase to obtain a polydopamine-coated molybdenum disulfide material;

[0008] 4. Polydopamine-coated molybdenum disulfide material, polyvinylidene fluoride and Ketjen black are uniformly mixed in a mass ratio of (8-9):1:1, and then N-methylpyrrolidone is added and mixed uniformly to obtain a slurry; the slurry is then applied to a titanium substrate and dried to obtain a capacitive deionization electrode for uranium solution enrichment.

[0009] Furthermore, the average pore size of the microporous membrane described in step 1 is 0.2 to 0.25 μm.

[0010] Furthermore, in step three, the mass ratio of MoS2 to polydopamine in the stripped MoS2 aqueous solution is 1:(1~24).

[0011] The application of the capacitor deionization electrode for uranium solution enrichment prepared by the above method is to assemble the capacitor deionization electrode for uranium solution enrichment into a capacitor deionization system to enrich uranium in the uranium-containing solution. The specific method is: two capacitor deionization electrodes for uranium solution enrichment are used as the positive and negative electrodes of the capacitor deionization device 1 respectively, wherein the spacing between the two capacitor deionization electrodes for uranium solution enrichment is 3 to 12 mm; then the electrodes of the capacitor deionization device 1 are respectively connected to the positive and negative electrodes of the power supply 2; and the uranium-containing The liquid outlet of the container 3 of the uranium solution is connected to the inlet of the capacitor deionization device 1 through the peristaltic pump 4; the outlet of the capacitor deionization device 1 is connected to the liquid inlet of the container 3 to obtain a capacitor deionization system; the uranium-containing solution is added to the container 3, and the uranium-containing solution is input into the capacitor deionization device 1 through the peristaltic pump 4, enriched under the condition of a voltage of 0.8 to 1.2 V, and then returned to the container from the outlet of the capacitor deionization device, and the uranium-containing solution is circulated and enriched for 300 to 800 minutes to complete the enrichment of uranium in the uranium-containing solution.

[0012] Furthermore, the uranium-containing solution contains uranyl ions (UO2 2+ ) and / or uranyl carbonate ions (UO2(CO3)2 2+ ).

[0013] Furthermore, the flow rate of the uranium-containing solution was 40 mL min-1 .

[0014] The first method for regenerating the capacitor deionization device after adsorption saturation is: open-circuiting or short-circuiting the capacitor deionization device 1, and circulating the uranium-containing solution for 10 to 15 minutes to complete the regeneration.

[0015] The second method for regenerating the capacitor deionization device after adsorption saturation is: first open or short-circuit the capacitor deionization device 1, and circulate the uranium-containing solution for 10 to 15 minutes; then, circulate it with 0.1M HNO3 for 20 minutes to complete the regeneration.

[0016] The present invention uses polydopamine to coat molybdenum disulfide with a thickness of 2.7 to 10.8 nm, so that the interface state of molybdenum disulfide changes significantly, the hydrophilicity is increased, and the adsorption of uranyl ions and / or uranyl carbonate ions in the uranium solution is greatly improved. When assembled into a capacitor deionization system for treating uranium solution, the uranium enrichment amount can be increased by 2 to 3 times, and the saturated adsorption capacity can be increased by 2 to 3 times compared with molybdenum disulfide. The capacitor deionization system after adsorption saturation can be regenerated and recycled for 5 times. The capacitor deionization electrode for uranium solution enrichment of the present invention can be used in the field of uranium-containing wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The microscopic morphology of MoS2 in Example 1;

[0018] Figure 2 The microscopic morphology of PDA@MoS2-2 in Example 1;

[0019] Figure 3 The microscopic morphology of PDA@MoS2-4 in Example 2;

[0020] Figure 4 The microscopic morphology of PDA@MoS2-12 in Example 3;

[0021] Figure 5 The microscopic morphology of PDA@MoS2-24 in Example 4;

[0022] Figure 6 is an atomic force microscope image of MoS2 in Example 1;

[0023] Figure 7 This is an atomic force microscope image of PDA@MoS2-2 in Example 1;

[0024] Figure 8 This is an atomic force microscope image of PDA@MoS2-4 in Example 2;

[0025] Fig. 9 This is an atomic force microscope image of PDA@MoS2-12 in Example 3;

[0026] Fig.10 This is an atomic force microscope image of PDA@MoS2-24 in Example 4;

[0027] Fig.11 is the contact angle between MoS2 and water in Example 1;

[0028] Fig.12 is the contact angle between PDA@MoS2-2 and water in Example 1;

[0029] Fig.13 is the contact angle between PDA@MoS2-4 and water in Example 2;

[0030] Fig.14 is the contact angle between PDA@MoS2-12 and water in Example 3;

[0031] Fig.15 is the contact angle between PDA@MoS2-24 and water in Example 4;

[0032] Fig.16 CV curves of the MoS2 electrode prepared in Comparative Example 1, the PDA@MoS2-2 electrode prepared in Example 1, the PDA@MoS2-4 electrode prepared in Example 2, the PDA@MoS2-12 electrode prepared in Example 3, and the PDA@MoS2-24 electrode prepared in Example 4;

[0033] Fig.17 This is a graph showing the electrochemical stability test results of the PDA@MoS2-4 electrode prepared in Example 2;

[0034] Fig.18 The constant current charge and discharge curves of the PDA@MoS2-4 electrode prepared in Example 2 at different current densities;

[0035] Fig.19 Schematic diagram of the structure of the capacitive deionization system; in the figure, 1 is a capacitive deionization device, 2 is a power supply, 3 is a container, and 4 is a peristaltic pump;

[0036] Fig. 20 The result diagram of the enrichment ability of MoS2 electrode, PDA@MoS2-4 electrode, PDA@MoS2-12 electrode and PDA@MoS2-24 electrode for uranium at different pH values ​​in Application Example 1;

[0037] Fig.21 It is the enrichment result diagram of MoS2 electrode, PDA@MoS2-2 electrode, PDA@MoS2-4 electrode, PDA@MoS2-12 electrode and PDA@MoS2-24 electrode in Application Example 1;

[0038] Fig. 22This is a graph showing the relationship between the enrichment rate of the PDA@MoS2-4 electrode and the voltage in Application Example 2;

[0039] Fig.23 is a curve diagram showing the relationship between the enrichment amount and time at different uranium solution circulation rates in Application Example 3;

[0040] Fig.24 is a graph showing the relationship between the adsorption amount and the electrode spacing in Application Example 4;

[0041] Fig.25 It is a diagram of the enrichment rate of each cycle of the electrode in Application Example 5;

[0042] Fig.26 The antibacterial relationship between the MoS2 electrode and the PDA@MoS2-4 electrode in Application Example 6;

[0043] Fig. 27 This is a graph showing the relationship between the enrichment of seawater by the PDA@MoS2-4 electrode in Application Example 7 and time. DETAILED DESCRIPTION

[0044] Use the following examples to verify the beneficial effects of the present invention:

[0045] Example 1: The preparation method of the capacitor deionization electrode for uranium solution enrichment of this Example 1 is carried out according to the following steps:

[0046] 1. Preparation of MoS2 powder: 2.48g (NH4)6Mo7O 24 4H2O and 4.56gCN2H4S were added to 72mL of deionized water, and ultrasonic treatment was performed for 30 minutes to obtain a uniform mixed solution. The mixed solution was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and hydrothermally treated at 200°C for 8h. After the reaction was completed, it was naturally cooled to room temperature, and vacuum filtered with a mixed cellulose microporous membrane with an average pore size of 0.22μm to collect the black precipitate, which was then washed 3 times with deionized water and then vacuum freeze-dried at -67°C to obtain MoS2 powder.

[0047] 2. Add 100 mg of MoS2 powder to 100 mL of Tris buffer solution at pH 8.5, and then put it into an ultrasonic cleaner for 30 minutes at a power of 100 W and a frequency of 30 kHz to obtain an exfoliated MoS2 aqueous solution;

[0048] 3. Add 100 mg of polydopamine (PDA) to the stripped MoS2 aqueous solution obtained in step 2, shake at 180 rpm for 2 h, filter, and freeze-dry the solid phase at -67 ° C to obtain a polydopamine-coated molybdenum disulfide material; record it as PDA@MoS2-2;

[0049] 4. 0.8 g polydopamine-coated molybdenum disulfide material, 0.1 g polyvinylidene fluoride and 0.1 g Ketjen black were uniformly mixed to obtain electrode material, and then 250 μL N-methylpyrrolidone was added and magnetically stirred for 8 h to obtain slurry; the slurry was then applied to the titanium substrate, where the mass of the electrode material was 10 mg and the active area was about 6.25 cm 2 , and then the titanium substrate coated with the slurry was placed in an oven at 60°C and dried for 10 h to obtain a capacitive deionization electrode for uranium solution enrichment, which was recorded as PDA@MoS2-2 electrode.

[0050] Example 2: The difference between this example and Example 1 is that the oscillation time in step three is 4 hours, and a polydopamine-coated molybdenum disulfide material is obtained; it is denoted as PDA@MoS2-4, and the other steps and parameters are the same as those in Example 1, and the obtained electrode is denoted as PDA@MoS2-4 electrode.

[0051] Example 3: The difference between this example and Example 1 is that the oscillation time in step three is 12 hours, and the polydopamine-coated molybdenum disulfide material is obtained; it is recorded as PDA@MoS2-12, and the other steps and parameters are the same as in Example 1, and the obtained electrode is recorded as PDA@MoS2-12 electrode.

[0052] Example 4: The difference between this example and Example 1 is that the oscillation time in step three is 24 hours, and the polydopamine-coated molybdenum disulfide material is obtained; it is recorded as PDA@MoS2-24, and the other steps and parameters are the same as in Example 1, and the obtained electrode is recorded as PDA@MoS2-24 electrode.

[0053] Comparative Example 1: This comparative example uses MoS2 powder to prepare an electrode, and the specific steps are as follows:

[0054] 1. Preparation of MoS2 powder: The specific preparation method is the same as step 1 of Example 1;

[0055] 2. MoS2 powder, polyvinylidene fluoride and Ketjen black were uniformly mixed in a mass ratio of 8:1:1, and 250uL N-methylpyrrolidone was added. The mixture was magnetically stirred for 8 hours to obtain a slurry. The slurry was then applied to a titanium substrate and dried in an oven at 60°C for 10 hours to obtain a capacitive deionization electrode for comparison, which was recorded as a MoS2 electrode.

[0056] The MoS2 powder prepared in step 1 of Example 1 and PDA@MoS2-2 prepared in step 3, PDA@MoS2-4 prepared in step 3 of Example 2, PDA@MoS2-12 prepared in step 3 of Example 3, and PDA@MoS2-24 prepared in step 3 of Example 4 were tested by scanning electron microscope, and the microscopic morphologies obtained were as follows: Figures 1 to 5 As shown, from Figure 1 From the microscopic scanning electron microscope image, it can be seen that MoS2 is a flower-like structure assembled by nanosheets. As the deposition time of PDA@MoS2 increases, more and more PDA is deposited on the surface, and it tends to aggregate together. By adjusting the oscillation time, the amount of PDA deposited on MoS2 can be controlled.

[0057] By atomic force microscopy, the surface information and coating thickness of the MoS2 powder prepared by step 1 in Example 1 and the PDA@MoS2-2 prepared by step 3, the PDA@MoS2-4 prepared by step 3 in Example 2, the PDA@MoS2-12 prepared by step 3 in Example 3, and the PDA@MoS2-24 prepared by step 3 in Example 4 were tested. The test results are as follows: Figures 6 to 10 As shown,

[0058] from Figure 6 It can be seen that the thickness of MoS2 nanosheets is 1.4 nm;

[0059] from Figure 7 It can be seen that the thickness of PDA@MoS2-2 is 4.1nm; it can be calculated that the thickness of PDA is 2.7nm.

[0060] from Figure 8 It can be seen that the thickness of PDA@MoS2-4 is 7.1nm; the thickness of PDA can be calculated to be 5.7nm.

[0061] from Fig. 9 It can be seen that the thickness of PDA@MoS2-12 is 9.7nm; the thickness of PDA can be calculated to be 8.3nm.

[0062] from Fig.10 It can be seen that the thickness of PDA@MoS2-24 is 12.2nm; the thickness of PDA can be calculated to be 10.8nm.

[0063] The contact angle / surface tension measuring instrument was used to test the contact angles of MoS2, PDA@MoS2-2, PDA@MoS2-4, PDA@MoS2-12, and PDA@MoS2-24 with water. The test results are as follows: Figures 11 to 15 As shown:

[0064] from Fig.11It can be seen that the contact angle of MoS2 with water is 71.2°;

[0065] from Fig.12 It can be seen that the contact angle of PDA@MoS2-2 with water is 67.1°;

[0066] from Fig.13 It can be seen that the thickness of PDA@MoS2-4 is 57.5°;

[0067] from Fig.14 It can be seen that the thickness of PDA@MoS2-12 is 47.6 nm;

[0068] from Fig.15 It can be seen that the thickness of PDA@MoS2-24 is 32.9 nm;

[0069] The electrochemical cyclic voltammetry (CV) method was used to test the electrochemical behavior of the MoS2 electrode and the PDA@MoS2-2 electrode, PDA@MoS2-4 electrode, PDA@MoS2-12 electrode, and PDA@MoS2-24 electrode, so as to predict their performance in the capacitive deionization process. At a scan rate of 50 mV / s, the CV test was performed on the MoS2 electrode and the PDA@MoS2-2 electrode, PDA@MoS2-4 electrode, PDA@MoS2-12 electrode, and PDA@MoS2-24 electrode. The results are shown in Figure 2. Fig.16 As shown, from Fig.16 It can be seen that the CV curve is a symmetrical rectangle, which is a typical double-layer capacitor. The integrated area of ​​the CV curves of the PDA@MoS2-2 electrode and the PDA@MoS2-4 electrode gradually increases, while that of the PDA@MoS2-12 electrode and the PDA@MoS2-24 electrode decreases, indicating that the PDA@MoS2-4 electrode has the best electrochemical performance.

[0070] The electrochemical stability of the PDA@MoS2-4 electrode was tested. Fig.17 As shown, from Fig.17 It can be seen that after 100 consecutive cycles, the CV curve still maintains its original shape and the specific capacitance basically remains at 95%. The results show that the PDA@MoS2-4 electrode has good electrochemical stability and cycle stability.

[0071] The constant current charge and discharge curves of PDA@MoS2-4 electrode at different current densities are shown in Figure 2. Fig.18 As shown, from Fig.18 It can be seen that at different current densities, the charge-discharge curves are asymmetric quasi-triangular, indicating that the PDA@MoS2-4 electrode has good reversibility and pseudocapacitive properties.

[0072] Application Example 1: Assemble a capacitive deionization system using the electrodes prepared in Examples 1 to 4 and Comparative Example 1: Use two electrodes as the positive and negative electrodes of the capacitive deionization device 1, respectively, and then connect the electrodes of the capacitive deionization device 1 to the positive and negative electrodes of the power supply 2, respectively; connect the liquid outlet of the container 3 containing the uranium solution to the inlet of the capacitive deionization device 1 through the peristaltic pump 4; connect the outlet of the capacitive deionization device 1 to the liquid inlet of the container 3, and obtain a capacitive deionization system. Fig.19 The distance between the two capacitor deionization electrodes is 3 mm, and the uranyl ions (UO2 2+ ) The uranium-containing solution with a concentration of 50 mg / g was adjusted to pH 2, 3, 4, 5, 6, 7, 8, and 9, respectively, and then heated at 40 mL min -1 The flow rate was input into the capacitive deionization device 1, and the enrichment was carried out for 330 minutes under the condition of voltage of 1.2V. The residual concentration of uranium contained in the simulated uranium-containing solution after treatment was determined by inductively coupled atomic emission spectrometer (ICP-OES) to obtain the equilibrium concentration of uranium. Then, according to the amount of adsorbent, the volume of uranium solution, the initial concentration of uranium and the equilibrium concentration, the adsorption amount and uranium removal efficiency were calculated. The results of the enrichment capacity of each electrode for uranium at different pH values ​​are shown in the following figure. Fig. 20 As shown, from Fig. 20 It can be seen that at pH = 5.0, the enrichment rate of PDA@MoS2-4 electrode is the highest, 212.0 mg / g -1 The enrichment rate of PDA@MoS2-2 electrode is second. The enrichment results of MoS2 electrode and PDA@MoS2-2 electrode, PDA@MoS2-4 electrode, PDA@MoS2-12 electrode, and PDA@MoS2-24 electrode for uranium solution with a concentration of 50 mg / g are shown in the figure. Fig.21 As shown, from Fig.21 It can be seen that the enrichment rate of PDA@MoS2-4 electrode is 99.9%.

[0073] Application Example 2: The PDA@MoS2-4 electrode prepared in Example 2 is used to assemble a capacitive deionization system, wherein the distance between the two capacitive deionization electrodes is 3 mm, and the uranyl ions (UO2 2+ ) concentration is 50 mg·L -1 The uranium-containing solution was adjusted to pH 5 and then -1The flow rate was input into the capacitive deionization system, and enriched for 900 minutes at voltages of 0, 0.2, 0.4, 0.6, 0.8, 1.0, and 1.2 V, respectively. The residual concentration of uranium contained in the simulated uranium-containing solution after treatment was determined by inductively coupled atomic emission spectrometry (ICP-OES) to obtain the equilibrium concentration of uranium; then, according to the amount of adsorbent, the volume of uranium solution, the initial concentration of uranium, and the equilibrium concentration, the adsorption amount and uranium removal efficiency were calculated. The relationship between the removal efficiency and the voltage is shown in the figure below: Fig. 22 As shown, from Fig. 22 It can be seen that when the applied voltage is 0V (open circuit voltage), UO2 2+ The enrichment rate is 27%. With the increase of the applied voltage, the enrichment rate gradually increases. The enrichment rate at 1.2V (81%) is three times that at 0V (27%).

[0074] Application Example 3: The PDA@MoS2-4 electrode prepared in Example 2 is used to assemble a capacitive deionization system, wherein the distance between the two capacitive deionization electrodes is 3 mm, and the uranyl ions (UO2 2+ ) concentration is 50 mg·L -1 The uranium-containing solution was adjusted to pH 5 and then heated at 10 mL min -1 、20mL·min -1 、30mL·min -1 、40mL·min -1 The flow rate was input into the capacitive deionization system, enriched at a voltage of 1.2V, and the residual concentration of uranium contained in the simulated uranium-containing solution after treatment was determined by inductively coupled atomic emission spectrometry (ICP-OES) to obtain the equilibrium concentration of uranium; then the adsorption amount was calculated based on the amount of adsorbent, the volume of uranium solution, the initial concentration of uranium and the equilibrium concentration. The relationship curve between enrichment amount and time at different uranium solution circulation rates is shown in the figure below: Fig.23 As shown by Fig.23 It can be seen that the circulation flow rate is 10mL·min -1 The electrosorption reached equilibrium at 600 min, and the circulation flow rate was 20 mL min -1 The electrosorption reached equilibrium at 540 min, and the circulation flow rate was 30 mL min -1 The electrosorption reached equilibrium at 400 min, and the circulation flow rate was 40 mL min -1 The electrosorption reached equilibrium at 330 min.

[0075] Application Example 4: A capacitive deionization system was assembled using the PDA@MoS2-4 electrode prepared in Example 2, wherein the spacing between the two capacitive deionization electrodes was 3 mm, 6 mm, 9 mm, and 12 mm, respectively, and uranyl ions (UO2 2+ ) concentration is 50 mg·L-1 The uranium-containing solution was adjusted to pH 5 and then -1 The flow rate was input into the capacitive deionization system, enriched under the condition of voltage of 1.2V, and the residual concentration of uranium contained in the simulated uranium-containing solution after treatment was determined by inductively coupled atomic emission spectrometry (ICP-OES) to obtain the equilibrium concentration of uranium; then the adsorption amount was calculated based on the amount of adsorbent, the volume of uranium solution, the initial concentration of uranium and the equilibrium concentration. The relationship between the adsorption amount and the electrode spacing is shown in the figure below: Fig.24 As shown, from Fig.24 It can be seen that when the electrode spacing is adjusted to 3mm, 6mm, 9mm, and 12mm, the corresponding enrichment rates are 81.23%, 58.41%, 46.98%, and 34.59%. As the electrode spacing increases, the enrichment rate gradually decreases.

[0076] Application Example 5: The PDA@MoS2-4 electrode prepared in Example 2 is used to assemble a capacitive deionization system, wherein the distance between the two capacitive deionization electrodes is 3 mm, and the uranyl ions (UO2 2+ ) concentration is 50 mg·L -1 The uranium-containing solution was adjusted to pH 5 and then -1 The flow rate is input into the capacitor deionization system, and the enrichment is carried out for 900 minutes under the condition of voltage of 1.2V. The first regeneration method of the capacitor deionization system after adsorption saturation is to open or short-circuit the capacitor deionization device 1, and circulate the uranium-containing solution for about 10 minutes to test the resolution rate. The resolution rate = test concentration / initial concentration, and the test concentration is the uranium concentration in the uranium-containing solution after the test cycle. The enrichment rate of each cycle is obtained as follows Fig.25 As shown, from Fig.25 It can be seen that through simple open circuit / short circuit (one-step desorption method), the PDA@MoS2-4 electrode has a resolution of 43.12% and a regeneration enrichment rate of 34.88% after 5 CDI cycles.

[0077] In addition, the second regeneration method of the capacitive deionization system after adsorption saturation is to open or short-circuit the CDI module and circulate the uranium-containing solution for about 10 minutes; then, 50ml of 0.1M HNO3 is circulated for 20 minutes. The test resolution is the sum of the two parts, resolution = test concentration / initial concentration, and the test concentration is the sum of the uranium concentration in the uranium-containing solution after the test cycle and the uranium concentration in the HNO3 solution after the test cycle. When the open / short circuit plus HNO3 elution two-step desorption method is used, the resolution is significantly improved. When the HNO3 concentration is 0.1M, the resolution of the PDA@MoS2-4 electrode reaches 65.45% after 5 CDI cycles, and the regeneration enrichment rate is 60.78%, with good regeneration performance.

[0078] Application Example 6: The antibacterial performance of the electrodes prepared in Example 2 and Comparative Example 1 against Escherichia coli and Staphylococcus aureus: Escherichia coli (ATCC 25922) and Staphylococcus aureus (ATCC 6538) were used as test bacteria, and the concentrations of the bacterial suspensions used in the test were 9.1×105 CFU / mL and 8.3×105 CFU / mL, respectively. The test was performed according to the GB / T 21510-2008 nano-inorganic material antibacterial performance test method (808nm laser irradiation). The control sample used the nano-silicon dioxide powder without antibacterial performance provided by the test party. The results are as follows: Fig.26 The suspension of Escherichia coli and Staphylococcus aureus are shown in Fig.26 As shown in the first row, the bacterial suspensions of Escherichia coli and Staphylococcus aureus after adding MoS2 and PDAs@MoS2-4, respectively, are as follows Fig.26 As shown in the second line, from Fig.26 It can be seen that the antibacterial rates of MoS2 prepared in comparative example 1 are 58.724% and 42.424%, respectively. The antibacterial rates of PDA@MoS2-4 prepared in example 2 are 99.998% and 99.997%, respectively.

[0079] Application Example 7: The PDA@MoS2-4 electrode prepared in Example 2 is used to assemble a capacitive deionization system, wherein the distance between the two capacitive deionization electrodes is 3 mm, and 20 L of natural seawater is pumped at 40 mL min by a peristaltic pump. -1 The flow rate of 1.2V was input into the capacitive deionization system, and uranium was enriched under the condition of 1.2V. The residual concentration of uranium contained in the simulated uranium-containing solution after treatment was measured by inductively coupled atomic emission spectrometer (ICP-OES) to obtain the equilibrium concentration of uranium. Then, the adsorption amount was calculated based on the amount of adsorbent, the volume of uranium solution, the initial concentration of uranium and the equilibrium concentration. The enrichment amount versus time relationship diagram is shown in the figure below: Fig. 27 As shown in Figure 27, the initial UO2 of seawater measured by ICP-MS 2+ The concentration is about 3.1ug·g -1 After 10 days of electrosorption, 6.136±0.15 mg·g -1 UO2 2+ Extraction volume.

Claims

1. A method for preparing a capacitive deionization electrode for uranium solution enrichment, characterized in that The method proceeds as follows:

1. Preparation of MoS2 powder: (NH4)6Mo7O 24 The molar ratio of 4H2O to CN2H4S is 1:

2. 24 4H2O and CN2H4S are added to deionized water, and after ultrasonic treatment, a uniform mixed solution is obtained; the mixed solution is then transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and hydrothermally treated at a temperature of 160-250°C for 6-8 hours; after the reaction is completed, it is naturally cooled to room temperature, and a black precipitate is collected by vacuum filtration with a microporous membrane, and then the precipitate is washed clean with deionized water, and then vacuum freeze-dried to obtain MoS2 powder; 2. Add MoS2 powder to a Tris buffer solution with a pH of 7 to 10, and then put it into an ultrasonic cleaner, and ultrasonically treat it for 30 to 60 minutes at a power of 100 to 200 W and a frequency of 30 to 60 kHz to obtain an exfoliated MoS2 aqueous solution; 3. Add polydopamine to the stripped MoS2 aqueous solution, shake at a speed of 180-200 rpm for 1-6 hours, filter, and freeze-dry the solid phase to obtain a polydopamine-coated molybdenum disulfide material; 4. Polydopamine-coated molybdenum disulfide material, polyvinylidene fluoride and Ketjen black are uniformly mixed in a mass ratio of (8-9):1:1, and then N-methylpyrrolidone is added and mixed uniformly to obtain a slurry; the slurry is then applied to a titanium substrate and dried to obtain a capacitive deionization electrode for uranium solution enrichment.

2. The method for preparing a capacitive deionization electrode for uranium solution enrichment according to claim 1, characterized in that: The average pore size of the microporous membrane described in step 1 is 0.2 to 0.25 μm.

3. The method for preparing a capacitive deionization electrode for uranium solution enrichment according to claim 1 or 2, characterized in that: In step three, the mass ratio of MoS2 to polydopamine in the stripped MoS2 aqueous solution is 1:(1-24).

4. Application of the capacitive deionization electrode for uranium solution enrichment prepared by the method of claim 1, characterized in that The application is to assemble the capacitive deionization electrodes used for uranium solution enrichment into a capacitive deionization system to enrich uranium in uranium-containing solution.

5. The use of a capacitive deionization electrode for uranium solution enrichment according to claim 4, characterized in that The capacitor deionization electrodes for enriching uranium solution are assembled into a capacitor deionization system. The method for enriching uranium in the uranium-containing solution is specifically as follows: two capacitor deionization electrodes for enriching uranium solution are used as the positive and negative electrodes of a capacitor deionization device (1), respectively, wherein the distance between the two capacitor deionization electrodes for enriching uranium solution is 3 to 12 mm; the electrodes of the capacitor deionization device (1) are respectively connected to the positive and negative electrodes of a power source (2); the liquid outlet of a container (3) containing the uranium-containing solution is connected to the positive and negative electrodes of a power source (2) through a peristaltic pump (4); The inlet of the capacitor deionization device (1) is connected; the outlet of the capacitor deionization device (1) is connected to the liquid inlet of the container (3), thereby obtaining a capacitor deionization system; a uranium-containing solution is added to the container (3), the uranium-containing solution is input into the capacitor deionization device (1) through a peristaltic pump (4), enriched under a voltage of 0.8 to 1.2 V, and then returned to the container (3) from the outlet of the capacitor deionization device (1), and the uranium-containing solution is circulated and enriched for 300 to 800 minutes, thereby completing the enrichment of uranium in the uranium-containing solution.

6. The use of a capacitive deionization electrode for uranium solution enrichment according to claim 5, characterized in that: The uranyl solution contains uranyl ions and / or uranyl carbonate ions.

7. The use of a capacitive deionization electrode for uranium solution enrichment according to claim 5, characterized in that: The flow rate of the uranium-containing solution is 40 mL min -1 .

Citation Information

Patent Citations

  • Polydopamine modified molybdenum disulfide composite silver nanoparticle antibacterial agent and preparation method thereof

    CN108478597A

  • Preparation method and application of carbon nanotube loaded phosphorus nitride electrode material

    CN115477372A

  • Flowing electrode, application and regeneration method thereof, and method for enriching uranium in uranium-containing water body by using flowing electrode capacitive deionization device

    CN117383666A

  • Organic light emitting display apparatus

    KR1020240120344A