Preparation method of hard X-ray zone plate

Through two-step photolithography and electroplating processes, the wave band area is divided, combined with high-precision alignment technology and optimized electroplating parameters, the problem of poor high uniformity of the hard X-ray wave band sheet electroplating layer is solved, and higher diffraction efficiency and stability are achieved , meets the needs of high-precision waveband processing.

CN118919123APending Publication Date: 2024-11-08UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411108905.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the high resolution hard X-ray wave band sheets have poor height uniformity in the electroplating layer during processing, and the height consistency of the inner ring wave band and the outer ring wave band metal is difficult to control, especially when the line width changes greatly, the metal after electroplating is The structural height varies greatly, affecting the diffraction efficiency.

Method used

Using a two-step manufacturing process, the wave band is divided into the outer and inner ring belt areas through high-precision lithography, and the metal structure height of each area is independently controlled by optimizing process parameters during the electroplating process, and the cursor is aligned with high precision. Monitor and adjust plating errors and step-by-step plating to improve plating uniformity.

Benefits of technology

Effectively reduce the metal height difference between the outer ring belt and the inner ring belt to 5%-6%, improve the diffraction efficiency by about 20%, and improve the stability of the processing technology, satisfying that the outer ring belt width is 30nm and the metal height is 500nm wave band processing requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919123A_ABST
    Figure CN118919123A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a hard X-ray zone plate, and belongs to the technical field of semiconductors, and the method comprises the following process steps: step 1, designing a zone plate structure exposure layout, and dividing the layout into two parts, namely an outer ring zone A region and an inner ring zone B region; meanwhile, overlay alignment marks C and verniers E1 and E2 for measuring alignment errors are added on the periphery of the zone plate structure area; 2, manufacturing a silicon nitride suspension film substrate required by the zone plate; 3, an outer ring belt A area structure is manufactured, and meanwhile an alignment mark C and an alignment vernier E1 structure are machined; 4, an alignment mark C is used for manufacturing an inner ring belt B area structure in an overlay mode, and meanwhile an alignment vernier E2 structure is machined; and 5, carrying out microscopic detection on the processing precision of the wave zone plate. According to the invention, the zone plate structure is manufactured by two steps of photoetching and electroplating, and wavebands with large line width difference of the zone plate are subjected to photoetching and electroplating separately, so that the height uniformity of the whole metal structure of the zone plate can be improved, and the diffraction efficiency is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano-processing, and in particular relates to a method for preparing a hard X-ray zone plate. Background Art

[0002] Fresnel zone plate is one of the key focusing and imaging elements of synchrotron radiation X-ray optical imaging system. The preparation process of zone plate usually includes electron beam lithography and electroplating process. Electron beam lithography is a high-resolution exposure technology that can meet the processing of fine structure of zone plate. The metallization of zone plate structure combined with electroplating process can improve the diffraction efficiency of diffractive optical element. The line width and height of the outer ring of zone plate are the key factors and determining factors that ultimately affect the resolution and diffraction efficiency of optical element. Therefore, it is of great significance to control the height of the overall metal structure of zone plate to improve the diffraction efficiency of zone plate. The difficulty of processing with one-step exposure and one-step electroplating pattern transfer process is that the height uniformity of electroplated metal layer is not good. This is mainly because the zone plate is a concentric ring structure with gradually increasing line width from outside to inside. During the electroplating process, chemical mass transfer and ion diffusion will change with the change of line width of zone plate ring. The greater the line width change, the greater the height difference of metal structure after electroplating. The height of outer ring band metal structure after electroplating will be 20%-30% lower than that of inner ring band metal structure. Although optimizing the electroplating process conditions can improve the uniformity of the electroplated layer to a certain extent, the improvement effect is limited for zone plates with large line width variations. Therefore, it is often difficult to ensure the high consistency of the metal structure during the processing of high-resolution hard X-ray zone plates. Summary of the invention

[0003] In order to solve the problem that the metal height uniformity of the electroplated layer is poor and the metal height consistency of the inner ring wave zone and the outer ring wave zone is difficult to control during the processing of high-resolution hard X-ray zone plates. The present invention provides a method for preparing hard X-ray zone plates. This process divides the zone plates of the same structure into two steps. Specifically, during photolithography, high-precision alignment technology is used to achieve precise exposure of the outer ring band and the inner ring band area, and a high-precision alignment cursor is made at the same time. After processing, the overlay error can be instantly read by the cursor; during electroplating, the outer ring wave band and the inner ring wave band with large line width variation are electroplated step by step, and the metal structure height of the inner ring band area and the outer ring band area is independently controlled by optimizing the electroplating process parameters to improve the uniformity of the coating. At present, the preparation method of the present invention can meet the processing requirements of zone plates with an outer ring wave band width of 30nm and a metal height of 500-550nm. Specifically, the following process steps are included: Step 1: Design the zone plate structure exposure layout, and divide the layout into two parts: the outer ring zone A area and the inner ring zone B area; at the same time, add the overlay alignment mark C around the zone plate structure area, and measure the cursors E1 and E2 of the alignment error; Step 2, making the silicon nitride suspension film substrate required for the zone plate; Step 3, making the outer ring belt A area structure, and processing the alignment mark C and alignment cursor E1 structure at the same time; Step 4: Use the alignment mark C to overlay and make the inner ring belt B area structure, and at the same time process the alignment cursor E2 structure; Step 5: Mirror inspection of the wave zone piece processing accuracy.

[0004] The present invention has the following beneficial technical effects: 1. The present invention divides the zone plate structure into two steps of photolithography and electroplating, separates the zone plates with large line width differences by photolithography and electroplating, and can improve the uniformity of the overall metal structure of the zone plate, and further improve the diffraction efficiency. The metal height difference between the outer ring and the inner ring can be reduced to 5%-6% by using this process to prepare a zone plate with a metal thickness of 500nm. After simulation, its diffraction efficiency can be improved by about 20%.

[0005] 2. The present invention divides the zone plate structure into two steps of exposure and electroplating. Considering that the precision of fine ring zone processing has a greater impact on the performance of optical components, the outer half ring zone of the zone plate is firstly made into a fine structure pattern, and then the inner ring zone pattern structure is processed by high-precision alignment technology. In order to quickly detect the overlay error, the zone plate is Figure 4 A high-precision detection alignment cursor is added to the peripheral area, and the alignment accuracy is monitored by reading the alignment cursor offset.

[0006] 3. The present invention divides the zone plate into two-step exposure and electroplating processing, which can improve the processing stability and meet the processing requirements of the zone plate with an outer ring band width of 30nm and a metal height of 500nm, while it is difficult to prepare it using a one-step photolithography and one-step electroplating process. The reasons are as follows: when a high-aspect ratio zone plate structure is made by a single-step photolithography and electroplating process, if it is to be ensured that the outer ring band metal height reaches 500nm during electroplating and the inner ring band metal structure is not over-plated, the overall electron beam photoresist thickness needs to be greater than 600nm. The increase in the thickness of the glue will aggravate the influence of the electron proximity effect during electron beam exposure, which is not conducive to the processing of high-resolution structures of 30nm and below; on the other hand, when processing the same line width band, the increase in the glue thickness will increase the depth-to-width ratio of the electron beam photoresist mask, and its mechanical properties will be weakened, which is not conducive to the electron beam photoresist structure remaining intact in the electroplating solution, and it is more likely to adhere and fall over. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1 A schematic diagram of a processing layout according to an embodiment of the present invention; Figure 2 is a schematic diagram of the three-dimensional structure of the silicon substrate layer; Figure 3 This is a schematic diagram of the structure after spin coating the first electron beam gel layer; Figure 4 It is a schematic diagram of the electron beam gel structure of the outer ring zone A area after development, the alignment mark C and the cursor E1 structure; Figure 5 It is a schematic diagram of the metal ring structure A, alignment mark C and cursor E1 structure after electroplating; Figure 6 It is a schematic diagram of the structure after the glue is evenly coated; Figure 7 It is a schematic diagram of the electron beam gel structure in the inner ring zone B area after development and the electron beam gel structure corresponding to the cursor E2; Figure 8 It is a schematic diagram of the metal structure of the inner ring belt B area and cursor E2 after electroplating; Fig. 9 It is a schematic diagram of the structure of the first electroplated metal layer 5 and the second electroplated metal layer 7 of the zone plate after debonding and the paired cursors E1 and E2.

[0008] In the figure: silicon substrate layer 1, silicon nitride suspension film layer 2, metal seed layer 3, first electron beam colloid layer 4, first electroplated metal layer 5, second electron beam colloid layer 6, second electroplated metal layer 7. DETAILED DESCRIPTION

[0009] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other. To achieve the above-mentioned purpose, the present invention adopts the following technical scheme.

[0010] The present invention provides a method for preparing a hard X-ray zone plate, which specifically comprises the following steps: Step 1: Design the exposure layout.

[0011] The zone plate is a variable-pitch concentric ring with a duty cycle of 1:1. The ring width increases from the outer ring to the inner ring. The ring width, number of rings and height are designed based on the line station focusing and imaging requirements. In this embodiment, the outermost ring width is 30nm, with a total of 1334 rings and a total diameter of 160um. Based on the requirements of high-precision alignment and zone plate applications, the layout is processed as follows: Step 1.1 See Figure 1 , the zone plate layout is divided into the outer ring zone A area and the inner ring zone B area. The radial width R1 of the outer ring zone A is 42um, the line width range is 30-60nm, and there are 1000 rings in total. It is a high-precision structural area, and its processing accuracy has a great influence on the performance of the zone plate. The radial width R2 of the inner ring zone B is 38um, the ring zone line width is 60nm-800nm, and there are 334 rings in total. Since the number of rings of the zone plate is too large to be fully shown in the figure, the number of middle rings is omitted, and the outer ring zone A area and the inner ring zone B area together constitute the complete structure of the zone plate.

[0012] Step 1.2 To meet the high-precision alignment requirements, add symmetrical alignment marks C at the intersection of four straight lines perpendicular to the X and Y axes 150um from the center of the zone plate. The alignment marks are in the shape of a "cross", with a length of 20-50um and a width of 3 microns. There are 4 marks. For specific distribution, see the schematic diagram. Figure 1 Middle C graphic.

[0013] Step 1.3 Design the overlay error detection cursor. Because the wave zone plate is fine in size, large processing errors will cause the two regional structures to focus eccentrically, which has a great impact on the performance of the optical element. In order to monitor the overlay accuracy, four pairs of cursors are added around the wave zone plate. The cursors can measure errors in the X and Y directions. The alignment cursor measurement resolution is 5nm. The projection area of ​​the cursor is within the range of the projection area of ​​the overlay alignment mark C. It is symmetrically distributed in the blank area around the wave zone plate pattern. There are 4 cursors. By averaging the overlay error measurement values ​​at the 4 positions, the influence of random errors on the measurement results is reduced. Cursors E1 and E2 are both a pair of vertical straight lines with a certain width; the cursors at the same position of the two pairs of cursors E1 and E2 are aligned and close together along the inner edges. See the schematic diagram and distribution of the cursor structure. Figure 1 Among E1 and E2, E1 and the graphics of area A of the outer ring are processed together, and E2 and the graphics of area B of the inner ring are processed together.

[0014] Step 2: Prepare the silicon nitride suspension film substrate required for the zone plate.

[0015] See also Figure 2 , a metal seed layer 3 is evaporated on the silicon nitride suspension film layer 2 supported by the silicon substrate layer 1. The thickness of the silicon nitride suspension film is 100nm, and the size of the silicon nitride suspension film window is 2mm 2mm square. Electron beam evaporation equipment is used to evaporate the metal seed layer 3 on the silicon nitride suspension film layer 2. The metal seed layer 3 is composed of metal chromium and gold from bottom to top, wherein the thickness of chromium is 5nm and the thickness of gold is 10nm. A high vacuum environment is required during the coating to ensure that the particle size of the metal is small enough.

[0016] Step 3: Make the outer ring band A metal, and at the same time process the alignment mark C and the alignment cursor E1 structure.

[0017] Step 3.1: Spin coating the first electron beam glue layer 4 on the metal seed layer 3. The electron beam glue component selected in this embodiment is polymethyl methacrylate, referred to as PMMA, with a molecular weight of 950K and a thickness of 500-550nm. The schematic diagram of the structure after the coating is shown in FIG. Figure 3 .

[0018] Step 3.2: Expose the outer band A pattern of the zone plate, and at the same time expose the alignment mark C and alignment vernier E1 outside the outer band A area. The electron beam lithography equipment used for exposure in this embodiment is Jeol 6300FS, with an acceleration voltage of 100kV and a beam spot size of 5nm. Because the line width of the outer band A area is fine and the processing accuracy is high, it is necessary to use appropriate exposure doses for different line width bands during exposure. The exposure dose of the outer band A pattern is 4000-5000uC / cm 2 The exposure dose of the cross mark C pattern is 2000uC / cm 2 , Cursor E1 pattern exposure dose is 3000uC / cm 2 Before exposure, the electron beam proximity effect was corrected using the commercial software Beamer and Tracer.

[0019] Step 3.3 Low-temperature development. Immerse the exposed substrate in a MIBK:IPA=1:3 solution for 60 seconds and fix with IPA for 30 seconds. The development temperature in this embodiment is 5°C. The advantage is that low-temperature development can improve the contrast of the electron beam gel and is more suitable for fine structure processing. After development, keep the sample wet and transfer it to deionized water for immersion for 2 minutes. After development, the outer ring A area ring electron beam gel structure, alignment mark C and cursor E1 structure schematic diagram can be seen in Figure 4 .

[0020] Step 3.4 Pulse electroplating. Transfer the substrate immersed in deionized water to the electroplating solution, keep the sample surface moist, and use the full water pulse electroplating technology to electroplate the first electroplated metal layer 5 in the structural gap of the first electron beam gel layer 4 after development. The specific electroplating conditions are as follows: electroplating temperature 50°C, current density 3.6A / dm 2 , the pulse duty cycle is 5%, the pulse frequency is 6000Hz, and the electroplating time is 8-9min to the preset thickness of 500nm. The schematic diagram of the metal ring structure A, alignment mark C and cursor E1 after electroplating can be seen in Figure 5 .

[0021] Step 4: Make the inner ring belt B metal structure and process the cursor E2 structure at the same time.

[0022] Step 4.1. Spin coating. After the substrate obtained in step 3.4 is cleaned with oxygen plasma for 1 minute, the overall thickness of the first electron beam glue layer 4 is thinned, and the second electron beam glue layer 6 is continuously spin-coated to a preset thickness. The first electron beam glue layer 4 does not need to be completely removed by oxygen plasma. It is sandwiched between the first electroplated metal layer 5 to buffer the impact of the spin coating of the second electron beam glue layer 6 on the first electroplated metal layer 5 with a large aspect ratio, thereby avoiding structural collapse. For a schematic diagram of the structure after spin coating, see Figure 6 .

[0023] Step 4.2: Use the four alignment marks C processed in step 3.4 to align and expose the inner ring band B of the zone plate, and process the vernier E2 structure at the same time. The specific exposure dose of the inner ring band B pattern is 3000-4000uC / cm 2 , Cursor E2 exposure dose is 3000uC / cm 2 .

[0024] Step 4.3 Low temperature development. The development conditions of this step are the same as those of step 3.3. After development, the electron beam gel structure of the inner ring zone B area and the electron beam gel structure corresponding to cursor E2 can be found in Figure 7 .

[0025] Step 4.4: Electroplating. The electroplating operation steps are the same as step 3.4. The second electroplated metal layer 7 is electroplated between the gaps between the first electron beam gel layer 4 and the second electron beam gel layer 6 after development. In order to control the structural height of the second electroplated metal layer 7 and the first electroplated metal layer 5 to be consistent, shortening the electroplating time of this step or reducing the current density can also achieve the same effect. After electroplating, the inner ring band B area and the cursor E2 metal structure can be seen in FIG. Figure 8 .

[0026] Step 4.5 Degumming. After the electroplating is completed, the sample is soaked in an organic reagent such as acetone for 5 minutes to remove the first electron beam glue layer 4 and the second electron beam glue layer 6. In order to avoid the adhesion and lodging of the high aspect ratio metal structure during drying, the carbon dioxide supercritical drying technology is used to obtain the complete zone plate metal structure. The structure of the first electroplated metal layer 5 and the second electroplated metal layer 7 of the zone plate after degumming and the paired cursor E1 and E2 are shown in Fig. 9 .

[0027] Step 5 is microscopic inspection, using a scanning electron microscope to characterize the zone plate overlay accuracy and metal height.

[0028] Step 5.1 Measure the metal height of the outermost ring zone A and the metal height of the inner ring zone B by scanning electron microscopy. When observing with the electron microscope, the substrate is tilted at a certain angle α to characterize the metal sidewall height h. The actual metal height after electroplating is h / sinα. The measurement found that the metal height difference between the inner and outer ring zones of the zone plate can be controlled within the range of 5%-6%. Step-by-step electroplating can better control the consistency of the overall metal height of the zone plate.

[0029] Step 5.2 Use a scanning electron microscope to characterize the E1 and E2 cursors and read the overlay errors in the X and Y directions. The overlay error read by the cursor is better than 20nm, which meets the requirements for the use of optical components.

Claims

1. A method for preparing a hard X-ray zone plate, It is characterized in that The method comprises the following process steps: Step 1: Design a zone plate structure exposure layout, and divide the layout into two parts: an outer ring zone A area and an inner ring zone B area; at the same time, set an overlay alignment mark C around the zone plate structure area, and measure the cursors E1 and E2 of the alignment error; Step 2, making the silicon nitride suspension film substrate required for the zone plate; Step 3, making the outer ring belt A area structure, and processing the alignment mark C and alignment cursor E1 structure at the same time; Step 4: Use the alignment mark C to overlay and make the inner ring belt B area structure, and at the same time process the alignment cursor E2; Step 5: Mirror inspection of the wave zone plate processing accuracy.

2. The method for preparing a hard X-ray zone plate according to claim 1, It is characterized in that The wave zone plate is a variable-pitch concentric ring with a duty cycle of 1:

1. The width of the ring increases from the outer ring to the inner ring. The inner ring zone B area is located inside the wave zone plate and extends a certain radial width outward from the center of the circle. The outer ring zone A area is located outside the inner ring zone B area and extends the remaining radial width outward from the outer edge of the inner ring zone B area; the radial width of the outer ring zone area A from the outside to the inside is greater than or equal to half the radius of the complete wave zone plate.

3. The method for preparing a hard X-ray zone plate according to claim 1, It is characterized in that In step 1, an overlay alignment mark C is symmetrically set at the intersection of four straight lines perpendicular to the X and Y axes at a certain distance from the center of the wave zone plate. The alignment mark is in a "cross" shape and there are four of them. Four pairs of vernier E1 and E2 are set around the wave zone plate. The vernier E1 and the vernier E2 are both a pair of perpendicular straight lines with a certain width. The verniers at the same position of the two pairs of vernier E1 and E2 are aligned and brought close to each other along the inner sides. The vernier is used to measure the error in the X and Y directions. The vernier measurement resolution is 5nm. The projection area of ​​the vernier is within the range of the projection area of ​​the overlay alignment mark C and is symmetrically distributed in the blank area around the wave zone plate pattern.

4. The method for preparing a hard X-ray zone plate according to claim 1, It is characterized in that The specific implementation method of step 2 is to evaporate a metal seed layer on the silicon nitride suspension film layer supported by the silicon substrate layer, and the size of the silicon nitride suspension film window is 2mm. 2mm square, electron beam evaporation equipment is used to evaporate a metal seed layer on the silicon nitride suspension film layer. The metal seed layer is composed of metal chromium and gold from bottom to top, with a chromium thickness of 5nm and a gold thickness of 10nm. A high vacuum environment is used during coating.

5. The method for preparing a hard X-ray zone plate according to claim 3, It is characterized in that Step 3 includes the following implementation steps: Step 3.1: Spin-coat the first electron beam glue layer on the metal seed layer. The electron beam glue component is polymethyl methacrylate, the molecular weight is 950K, and the thickness is 500-550nm; Step 3.2: Expose the outer ring zone A pattern of the zone plate, and simultaneously expose the alignment mark C and the alignment cursor E1 outside the outer ring zone A area; Step 3.3 Low-temperature development: immerse the exposed substrate in a MIBK:IPA=1:3 solution for 60 seconds, fix with IPA for 30 seconds, and after development, transfer the substrate to deionized water for immersion for 2 minutes while keeping it wet; Step 3.4: Pulse plating; The substrate immersed in deionized water is transferred to the electroplating solution, the substrate surface is kept moist, and the first electroplating metal layer is electroplated in the structural gaps of the first electron beam gel layer after development using all-water pulse electroplating technology; the specific electroplating conditions are as follows: electroplating temperature 50°C, current density 3.6A / dm2, pulse duty cycle 5%, pulse frequency 6000Hz, and electroplating to a preset thickness of 500nm.

6. The method for preparing a hard X-ray zone plate according to claim 5, It is characterized in that Step 4 includes the following implementation steps, specifically: Step 4.1: Spin coating; after cleaning the substrate obtained in step 3.4 with oxygen plasma, the overall thickness of the first electron beam glue layer is thinned, and the second electron beam glue layer is spin-coated to a preset thickness; Step 4.2 Use four alignment marks C to align and expose the inner ring band B of the zone plate, and process the vernier E2 structure at the same time; the specific exposure dose of the inner ring band B pattern is 3000-4000uC / cm 2 , Cursor E2 exposure dose is 3000uC / cm 2 ; Step 4.3 low temperature development; Step 4.4 electroplating: electroplating a second electroplated metal layer between the gaps between the first electron beam gel layer and the second electron beam gel layer after development, and controlling the second electroplated metal layer to have the same structural height as the first electroplated metal layer; Step 4.5: Remove the glue; after the electroplating is completed, remove the first electron beam glue layer and the second electron beam glue layer, and use carbon dioxide supercritical drying to obtain the first electroplated metal layer and the second electroplated metal layer structure of the wave zone plate.

7. The method for preparing a hard X-ray zone plate according to claim 6, It is characterized in that Step 5 includes the following implementation steps, specifically, Step 5.1 Measure the metal height of the outer ring zone A area and the metal height of the inner ring zone B area by scanning electron microscopy; when observing with the scanning electron microscope, the substrate is tilted at a certain angle α to characterize the side wall height h. The actual metal height after electroplating is h / sinα. The height difference of the metal between the inner and outer ring zones of the zone plate is controlled within the range of 5%-6%. Step 5.2: Use a scanning electron microscope to characterize the cursors E1 and E2, read the overlay error in the X direction and the Y direction, and the overlay error read by the cursor is better than 20nm.

8. The method for preparing a hard X-ray zone plate according to claim 4, It is characterized in that In step 2, the thickness of the silicon nitride suspension film is 100-200 nm, and the silicon nitride material is low stress.

9. The method for preparing a hard X-ray zone plate according to claim 1, It is characterized in that In step 3, when exposing the structure of the outer ring zone A area, the proximity effect of the electron beam is corrected; during development, a low-temperature development process is used, and the developer temperature is 0-5°C; during electroplating, the electroplating process parameters are controlled, including the use of pulse electroplating, appropriate current density and electroplating time.

10. The method for preparing a hard X-ray zone plate according to claim 1, It is characterized in that In step 4, area A is completely covered with electron beam glue during the uniform coating process; four overlay marks C are used for alignment during the overlay processing of area B, and at the same time, the metal height of area A in the outer ring belt and the metal height of area B in the inner ring belt are controlled to be basically consistent.