Insulated coated soft magnetic powder and preparation method and application thereof

Through a simplified environmentally friendly preparation method, the complex and pollution problems of insulating-covered soft magnetic powders in the prior art are solved, and the excellent salt spray resistance and pressure resistance of insulating-covered soft magnetic powders are achieved, which improves the The performance of inductors is suitable for complex environments.

CN118919277APending Publication Date: 2024-11-08HUIZHOU POCO IND CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411239571.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has the risk of environmental pollution and complex processes when preparing insulated coated soft magnetic powders, making it difficult to achieve excellent salt spray resistance and pressure resistance in large-scale production.

Method used

Using a simplified preparation method, the soft magnetic powder is premixed and dried with the main insulating agent and the auxiliary insulating agent using environmentally friendly reagents, and then mixed with the resin for granulation and drying to obtain an insulated coated soft magnetic powder, which is not required for the process. Washing steps.

Benefits of technology

It realizes excellent salt spray resistance, voltage resistance and rust resistance of insulated coated soft magnetic powder, improves the inductance value and DC biasing ability of the inductance, and is suitable for high frequency, high current and high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919277A_ABST
    Figure CN118919277A_ABST
Patent Text Reader

Abstract

The invention provides insulation coated soft magnetic powder and a preparation method and application thereof.The preparation method of the insulation coated soft magnetic powder comprises the steps that soft magnetic powder and a main insulating agent are premixed in a solvent A, then an auxiliary insulating agent is added for mixing and drying, and an intermediate product is obtained; and mixing the obtained intermediate product and resin in a solvent B, granulating and drying to obtain the insulated coated soft magnetic powder, the reagents used in the preparation method are environment-friendly and pollution-free, the preparation process is simple, post-treatment steps such as water washing are not needed, and meanwhile, the prepared insulated coated soft magnetic powder has excellent anti-rust performance, pressure resistance and salt spray resistance and is suitable for industrial production. And the further manufactured integrated inductor can be ensured to have a relatively high inductance value and a relatively strong direct current bias capability, and is more suitable for being used in a high-frequency and large-current environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inductance, and in particular relates to an insulating coated soft magnetic powder and a preparation method and application thereof. Background Art

[0002] Compared with traditional coil inductors, one-piece molded inductors have smaller size, higher integration, higher transmission efficiency, etc. By adopting unique structure and materials, they can achieve lower energy loss and higher magnetic coupling efficiency, thereby improving the overall performance of the electronic system. In addition, it must also have stronger high temperature resistance and anti-environmental interference capabilities so that it can be used normally in more complex working environments. As one of the important electronic components in electronic products, it is designed to meet the requirements of electronic products for small size and high performance. It has also been rapidly developed and widely used in the context of high-tech iteration.

[0003] At present, the raw materials of one-piece molded inductors are mostly soft magnetic materials. In order to increase their saturation magnetic induction intensity, the amount of silicon and chromium added to the raw materials will be reduced, which will have a negative impact on the anti-rust and insulation effect of the soft magnetic powder, so it needs to be treated with anti-rust coating. For example, CN114068123A discloses a soft magnetic powder composite, a magnetic powder core material and an insulating coating method based on organic growth. The soft magnetic powder composite provided by the invention includes a soft magnetic powder and an insulating coating layer, wherein the insulating coating layer wraps the soft magnetic powder; the material of the insulating coating layer is prepared by the cross-linking reaction of dopamine hydrochloride and polyethyleneimine; the soft magnetic powder is selected from metal and / or alloy materials containing Fe elements. The coating method provided by the invention has low hazard, can achieve high stability within a certain temperature range, has thin sizing and controllability of the insulating film thickness, high film uniformity, and effectively isolates eddy currents between particles; at the same time, the insulating coating layer has high adhesion, can reduce the amount of insulating adhesive used, is easy to press and form, reduces the dilution effect of the non-magnetic phase, and further improves the magnetic properties of the matrix; however, the preparation method provided by the invention requires the use of Tris-HCl buffer solution in the preparation process, and the pH needs to be adjusted accordingly, which affects large-scale production and poses risks of environmental pollution.

[0004] Therefore, in response to the above technical problems, developing a preparation method for an insulating coated soft magnetic powder that is simple to operate, pollution-free and can produce good insulation, excellent salt spray resistance and excellent pressure resistance is still a technical problem that needs to be urgently solved in this field. Summary of the invention

[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide an insulating coated soft magnetic powder and a preparation method and application thereof. The reagents used in the preparation method are all environmentally friendly, and the preparation process is simple, without the need for post-processing steps such as water washing. At the same time, the prepared insulating coated soft magnetic powder has excellent rust resistance, voltage resistance and salt spray resistance. After being further made into an integrated inductor, it also has a higher inductance value and stronger DC bias capability, and is more suitable for use in high frequency and high current environments.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing an insulating coated soft magnetic powder, the preparation method comprising the following steps:

[0008] (1) premixing the soft magnetic powder and the main insulating agent in solvent A, adding the auxiliary insulating agent, mixing, and drying to obtain an intermediate product;

[0009] (2) The intermediate product obtained in step (1) and the resin are mixed in solvent B, and the mixture is granulated and dried to obtain the insulating coated soft magnetic powder.

[0010] The preparation method provided by the present invention uses fewer types of insulating raw materials, which are all environmentally friendly and will not pose a risk of polluting the environment. At the same time, the overall process of the preparation method provided by the present invention is relatively simple, and no post-processing operations such as water washing are required, so it is suitable for mass production applications. In addition, the insulating coated soft magnetic powder prepared by the preparation method provided by the present invention has excellent comprehensive performance, excellent salt spray resistance, pressure resistance and rust resistance, and after being further made into an integrated inductor, the obtained integrated inductor has excellent rust resistance before and after reflow soldering and in a high temperature environment, and at the same time has strong pressure resistance, has little effect on the initial inductance value, improves the inductance value at 200Oe, enhances the DC bias capability, and is more suitable for complex environments with high frequency, high current and high temperature.

[0011] Preferably, the soft magnetic powder comprises gas atomized iron silicon chromium powder.

[0012] Preferably, the D of the soft magnetic powder 50 The particle size is 10 to 20 μm, for example, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm or 20 μm.

[0013] Preferably, based on the mass of the soft magnetic powder as 100g, the amount of the main insulating agent is 0.1-0.6g, for example, 0.1g, 0.2g, 0.3g, 0.4g, 0.5g or 0.6g, etc.; if the amount of the main insulating agent is too little, it is easy to cause the voltage resistance and rust resistance of the obtained insulating coated soft magnetic powder to decrease; if the amount of the main insulating agent is too high, it is easy to cause the inductance of the obtained insulating coated soft magnetic powder to decrease, thereby reducing the magnetic permeability of the magnetic core.

[0014] Preferably, the main insulating agent includes a main material and an auxiliary material; the main material includes any one of phytic acid, citric acid, acetic acid, nitrilotriacetic acid, 2-hydroxyethylethylenediaminetriacetic acid, diethylenetriaminepentaacetic acid, tartaric acid, aluminum dihydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, ethylenediaminetetrapropionic acid, sodium molybdate, gallic acid, tannic acid, boric acid or polyacrylic acid, or a combination of at least two of them; the auxiliary material includes any one of aluminum oxide, zinc oxide, magnesium oxide, calcium oxide, hydroxyapatite, magnesium hydroxide, zinc hydroxide, hydrophilic silica, hydrophobic silica, titanium dioxide, iron oxide or aluminum tripolyphosphate, or a combination of at least two of them; the above-mentioned specific types of main materials and specific types of auxiliary materials are used in combination as the main insulating agent, and the two can form a chemical conversion film on the surface of the magnetic powder, and the auxiliary material has a higher pressure resistance, and the film formed after compounding with the main material is hydrophobic and dense, and the surface resistance of the soft magnetic powder can also be increased.

[0015] Preferably, the mass ratio of the main ingredient to the auxiliary material is (1-4):1, for example, 1:1, 1.5:1, 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1 or 4:1, etc.

[0016] Preferably, based on the mass of the soft magnetic powder as 100g, the amount of the auxiliary insulating agent used is 0.1-0.5g, for example, 0.1g, 0.15g, 0.2g, 0.25g, 0.3g, 0.35g, 0.4g, 0.45g or 0.5g, etc.; if the amount of the auxiliary insulating agent used is too small, it is easy to cause the anti-rust effect of the obtained insulating coated soft powder to decrease; if the amount of the auxiliary insulating agent used is too high, it is easy to cause the pressing performance of the insulating coated soft powder to deteriorate (density decreases), and then cause the magnetic permeability to decrease.

[0017] Preferably, the auxiliary insulating agent includes any one or a combination of at least two of sodium silicate, silica sol, high base sodium sulfonate, boric acid amine, sodium benzoate, alkylphenol polyoxyethylene ether, fatty acid amide, alkyl alcohol amide, polyoxyethylene nonionic surfactant or polyoxyethylene amide.

[0018] Preferably, based on 100 g of the soft magnetic powder, the amount of the solvent A is 10 to 20 g, for example, 10 g, 12 g, 14 g, 16 g, 18 g or 20 g.

[0019] Preferably, the solvent A comprises any one of ethanol, xylene, acetone, ethyl acetate, propylene glycol, glycerol, deionized water, propanol or butanol, or a combination of at least two thereof.

[0020] Preferably, the premixing temperature in step (1) is 40-95°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 70°C, 80°C, 90°C or 95°C.

[0021] Preferably, the premixing time in step (1) is 5 to 60 min, for example, 5 min, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0022] Preferably, the mixing temperature in step (1) is 40-95°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 70°C, 80°C, 90°C or 95°C.

[0023] Preferably, the mixing time in step (1) is 5 to 60 min, for example, 5 min, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0024] Preferably, the drying temperature in step (1) is 80-250°C, for example, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C or 250°C.

[0025] Preferably, the drying time in step (1) is 30 to 180 min, for example, 30 min, 50 min, 70 min, 90 min, 110 min, 130 min or 150 min.

[0026] Preferably, based on 100 g of the soft magnetic powder, the amount of the resin is 1 to 3.5 g, for example, 1 g, 1.2 g, 1.4 g, 1.6 g, 1.8 g, 2 g, 2.2 g, 2.4 g or 2.5 g.

[0027] Preferably, the resin includes any one of epoxy resin, silicone resin, phenolic resin, urea-formaldehyde resin, ketone-alcohol resin, acrylic resin or polyimide resin, or a combination of at least two thereof.

[0028] Preferably, based on 100 g of the soft magnetic powder, the amount of the solvent B is 10 to 20 g, for example, 10 g, 12 g, 14 g, 16 g, 18 g or 20 g.

[0029] Preferably, the solvent B includes any one of ethanol, xylene, acetone, ethyl acetate, propylene glycol, glycerol, deionized water, propanol or butanol, or a combination of at least two thereof.

[0030] As a preferred technical solution, the preparation method comprises the following steps:

[0031] (1) premixing the soft magnetic powder, the main insulating agent and the solvent A at 40 to 95° C. for 5 to 60 minutes, adding the auxiliary insulating agent and continuing to mix at 40 to 95° C. for 5 to 60 minutes, and then drying at 80 to 250° C. for 30 to 180 minutes to obtain an intermediate product;

[0032] (2) The intermediate product obtained in step (1) and the resin are mixed in solvent B, and the mixture is granulated and dried to obtain the insulating coated soft magnetic powder.

[0033] In a second aspect, the present invention provides an insulating coated soft magnetic powder, wherein the insulating coated soft magnetic powder is prepared by the preparation method described in the first aspect.

[0034] In a third aspect, the present invention provides an integrally formed inductor, wherein the integrally formed inductor is obtained by pressing the insulating coated soft magnetic powder as described in the second aspect.

[0035] In a fourth aspect, the present invention provides a use of the insulating coated soft magnetic powder as described in the second aspect or the integrally formed inductor as described in the third aspect in electronic components.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] (1) The method for preparing the insulating coated soft magnetic powder provided by the present invention uses fewer types of raw materials, all of which are environmentally friendly, and thus will not pose a risk of polluting the environment;

[0038] (2) The overall process of the preparation method provided by the present invention is relatively simple, and no post-processing operations such as water washing are required, which is more suitable for mass production applications;

[0039] (3) The insulating coated soft magnetic powder prepared by the preparation method provided by the present invention has excellent comprehensive performance, including excellent salt spray resistance, pressure resistance and rust resistance. The integrated inductor further prepared has excellent rust resistance before and after reflow soldering and in high temperature environment. At the same time, it has strong pressure resistance and little effect on the initial inductance. The inductance value at 200Oe is higher, and the DC bias capability is enhanced, which is more suitable for use in complex environments with high frequency, large current and high temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1This is a photo of a magnetic ring made of the insulating coated soft magnetic powder provided in Example 1 before reflow soldering;

[0041] Figure 2 This is a photo of the magnetic ring made of the insulating coated soft magnetic powder provided in Example 1 after reflow soldering. DETAILED DESCRIPTION

[0042] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0043] Unless otherwise specified, the raw materials involved in the following specific embodiments are all existing materials and can be purchased commercially.

[0044] Example 1

[0045] A method for preparing an insulating coated soft magnetic powder comprises the following steps:

[0046] (1) Take 100g of atomized FeSiCr powder (D 50 The particle size is 15 μm), 0.5 g of a main insulating agent (composed of phytic acid, boric acid, sodium molybdate, acetic acid, calcium oxide, aluminum oxide and magnesium oxide in a mass ratio of 1:2:2:1:1:0.5:0.5) and 15 g of a mixed solvent (composed of deionized water and ethanol in a mass ratio of 7:3) are added, the mixture is placed in a water bath at 50° C. and mechanically stirred for 30 min, 0.2 g of alkyl alcohol amide is added, and the mixture is continued to be stirred and mixed in a water bath at 50° C. for 30 min, and after being stirred to a loose and dry state, the mixture is placed in an oven at 200° C. and baked for 100 min to obtain an intermediate product;

[0047] (2) The intermediate product obtained in step (1) and 2 g of epoxy resin (purchased from Nantong Xingchen, brand E51) are mixed in 15 g of ethanol, granulated and dried to obtain the insulating coated soft powder.

[0048] Example 2

[0049] A method for preparing an insulating coated soft magnetic powder comprises the following steps:

[0050] (1) Take 100g of atomized FeSiCr powder (D 50The mixture was placed in a water bath at 80°C with mechanical stirring for 20 min, and then 0.3 g of sodium silicate was added, and the mixture was stirred in a water bath at 80°C for 20 min. After stirring until the mixture was loose and dry, the mixture was placed in an oven at 100°C for 200 min to obtain an intermediate product.

[0051] (2) The intermediate product obtained in step (1) and 1.5 g of silicone resin (purchased from Dow Corning, brand SN-0806) are mixed in 10 g of ethanol, granulated and dried to obtain the insulating coated soft powder.

[0052] Example 3

[0053] A method for preparing an insulating coated soft magnetic powder comprises the following steps:

[0054] (1) Take 100g of atomized FeSiCr powder (D 50 The particle size is 15 μm), 0.4 g of a main insulating agent (mixed with citric acid, boric acid and hydrophobic silica in a mass ratio of 1:1:1) and 18 g of ethanol are added, the mixture is placed in a 90°C water bath and mechanically stirred for 10 min, and then 0.4 g of silica sol is added, and the mixture is stirred and mixed in a 90°C water bath for 10 min. After stirring until it is loose and dry, it is placed in an oven at 240°C and baked for 40 min to obtain an intermediate product;

[0055] (2) The intermediate product obtained in step (1) and 3 g of phenolic resin (purchased from Wuxi Jiunai Anticorrosion Materials Co., Ltd., brand 2130) are mixed in 20 g of ethanol, granulated and dried to obtain the insulating coated soft powder.

[0056] Embodiments 4 to 7

[0057] A method for preparing an insulating coated soft magnetic powder, which differs from Example 1 in that the amounts of the main insulating agent used are 0.1g (Example 4), 0.6g (Example 5), 0.05g (Example 6) and 0.7g (Example 7), respectively, and other substances, amounts and steps are the same as those in Example 1.

[0058] Embodiments 8 to 11

[0059] A method for preparing an insulating coated soft magnetic powder, which differs from Example 1 in that the amounts of alkyl alcohol amide used are 0.1g (Example 8), 0.5g (Example 9), 0.05g (Example 10) and 0.6g (Example 11), respectively, and other substances, amounts and steps are the same as those in Example 1.

[0060] Example 12

[0061] A method for preparing an insulating coated soft magnetic powder, which differs from Example 1 in that calcium oxide, aluminum oxide and magnesium oxide are not added, and other substances, amounts and steps are the same as those in Example 1.

[0062] Comparative Example 1

[0063] A method for preparing an insulating coated soft magnetic powder, comprising: atomizing FeSiCr powder (D 50 The coated aerosolized FeSiCr powder is obtained by mixing 2 g of an epoxy resin (purchased from Nantong Xingchen, with a particle size of 15 μm) and 2 g of an epoxy resin (purchased from Nantong Xingchen, with a brand name of E51) in 15 g of ethanol, granulating and drying.

[0064] Comparative Example 2

[0065] A method for preparing an insulating coated soft magnetic powder comprises the following steps:

[0066] (1) Take 100g of atomized FeSiCr powder (D 50 The particle size is 15 μm), 0.5 g of a main insulating agent (mixed with phytic acid, boric acid, sodium molybdate, acetic acid, calcium oxide, aluminum oxide and magnesium oxide in a mass ratio of 1:2:2:1:1:0.5:0.5) and 15 g of ethanol are added, the mixture is placed in a 50°C water bath and mechanically stirred for 30 min, and after being stirred to a loose and dry state, it is placed in an oven at 200°C and baked for 100 min to obtain an intermediate product;

[0067] (2) The intermediate product obtained in step (1) and 2 g of epoxy resin (purchased from Nantong Xingchen, brand E51) are mixed in 15 g of ethanol, granulated and dried to obtain the insulating coated soft powder.

[0068] Comparative Example 3

[0069] A method for preparing an insulating coated soft magnetic powder comprises the following steps:

[0070] (1) Take 100g of atomized FeSiCr powder (D 50 The particle size is 15 μm), 0.2 g of alkyl alcohol amide is added, and the mixture is stirred in a water bath at 50° C. for 30 min. After stirring until the mixture is loose and dry, the mixture is placed in an oven at 200° C. for 100 min to obtain an intermediate product.

[0071] (2) The intermediate product obtained in step (1) and 2 g of epoxy resin (purchased from Nantong Xingchen, brand E51) are mixed in 15 g of ethanol, granulated and dried to obtain the insulating coated soft powder.

[0072] Performance Test:

[0073] The coated soft magnetic powders provided in the examples and comparative examples were pressed at 600 MPa and room temperature, and the following tests were performed after the magnetic ring samples were obtained:

[0074] (1) Magnetic permeability: The inductance of the wound magnetic ring was measured using a MICROTEST 6632 impedance analyzer. Specifically, 26 turns of 0.7 mm diameter enameled copper wire were used for winding. The test frequency was 100 kHz, the voltage was 1 V, and the test temperature was room temperature 25°C. The initial inductance L was measured without DC bias. The magnetic permeability was then calculated using the following formula:

[0075]

[0076] Among them, le is the effective magnetic circuit length, N is the number of coil turns, and Ae is the effective magnetic circuit cross-sectional area.

[0077] (2) L (200 Oe) and DC (200 Oe): tested on the same impedance analyzer, bias current was applied according to the number of turns to test the inductance, the test frequency was 100 kHz, the voltage was 1 V, and the test temperature was room temperature 25°C.

[0078] (3) Reflow soldering voltage resistance: Use HIOKI SM7110 high resistance meter to test the 100V resistance value of the magnetic ring (the resistance value reflects the voltage resistance strength).

[0079] (4) Salt spray resistance: neutral salt spray for 24 hours, tested according to the test method provided in GB / T 2423.17-2008, reflow soldering simulation temperature is 260°C (maximum temperature time is 10 seconds, and the duration of the interval above 150°C is 10 minutes). The salt spray photos after reflow soldering refer to the photos after 4 salt spray cycles;

[0080] The photo of the magnetic ring made of the insulating coated soft magnetic powder provided in Example 1 before reflow soldering is as follows: Figure 1 As shown in the picture after reflow soldering Figure 2 As shown, according to Figure 1 and Figure 2 It can be seen from the comparison that the magnetic ring made of the insulating coated soft magnetic powder provided in Example 1 has no rust before and after reflow soldering, indicating that the insulating coated soft magnetic powder provided in Example 1 has excellent salt spray resistance.

[0081] The insulating coated soft magnetic powders provided in Examples 1 to 12 and Comparative Examples 1 to 3 were tested according to the above test method. The test results are shown in Table 1:

[0082] Table 1

[0083]

[0084] From the data in Table 1, we can see that:

[0085] (1) The magnetic permeability of the insulating coated soft magnetic powder provided in Examples 1 to 5 and Examples 8 to 9 after being made into a magnetic ring is 22.98 to 24.41 H / m, the initial inductance is as high as 8.96 to 9.52 μH, the inductance value is as high as 6.56 to 6.60 μH at 200 Oe, the DC bias is 68.91 to 73.21%, the withstand voltage after 0 reflow soldering is 88 to 363 Ω, and the withstand voltage after 4 reflow soldering is still as high as 96 to 298 Ω, and no rust is found before and after reflow soldering, indicating that the insulating coated soft magnetic powder provided in Examples 1 to 5 and Examples 8 to 9 has high inductance, excellent rust resistance, voltage resistance and salt spray resistance.

[0086] (2) Compared with Example 1, the preparation method provided in Comparative Example 1 does not add the main insulating agent and the auxiliary insulating agent, resulting in a relatively low inductance value of the obtained coated aerosolized FeSiCr powder, and poor pressure resistance and salt spray resistance.

[0087] (3) Compared with Example 1, no auxiliary insulating agent was added in the preparation method provided in Comparative Example 2, resulting in poor pressure resistance and salt spray resistance of the obtained insulating coated soft powder, and a significant decrease in inductance.

[0088] (4) Compared with Example 1, the preparation method provided in Comparative Example 3 does not add the main insulating agent, which also results in the obtained insulating coated soft powder having a relatively low inductance value, and poor pressure resistance and salt spray resistance.

[0089] (5) Compared with Example 1, the preparation method provided in Example 6 has an adverse effect on the pressure resistance and rust resistance of the obtained insulating coated soft magnetic powder due to the relatively small amount of main insulating agent used; while the preparation method provided in Example 7 has an adverse effect on the inductance of the obtained insulating coated soft magnetic powder due to the relatively large amount of main insulating agent used.

[0090] (6) Compared with Example 1, the preparation method provided in Example 10 has an adverse effect on the pressure resistance and rust resistance of the obtained insulating coated soft magnetic powder due to the relatively small amount of auxiliary insulating agent used; while the preparation method provided in Example 11 has an adverse effect on the inductance of the obtained insulating coated soft magnetic powder due to the relatively large amount of auxiliary insulating agent used.

[0091] (7) Finally, by comparing Example 1 and Example 12, it can be seen that the auxiliary materials in the main insulating agent are also equally important. The lack of auxiliary materials will also lead to a decrease in the pressure resistance and rust resistance of the obtained insulating coated soft magnetic powder.

[0092] The applicant declares that the present invention illustrates an insulating coated soft magnetic powder and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an insulating coated soft magnetic powder, It is characterized in that The preparation method comprises the following steps: (1) premixing the soft magnetic powder and the main insulating agent in solvent A, adding the auxiliary insulating agent, mixing, and drying to obtain an intermediate product; (2) The intermediate product obtained in step (1) and the resin are mixed in solvent B, and the mixture is granulated and dried to obtain the insulating coated soft magnetic powder.

2. The preparation method according to claim 1, It is characterized in that The soft magnetic powder includes aerosolized iron silicon chromium powder; Preferably, the gas atomized iron-silicon-chromium powder has a D 50 The particle size is 10~20μm.

3. The preparation method according to claim 1 or 2, It is characterized in that Based on the mass of the soft magnetic powder being 100 g, the amount of the main insulating agent is 0.1 to 0.6 g; Preferably, the main insulating agent comprises a main material and an auxiliary material; The main ingredients include any one or a combination of at least two of phytic acid, citric acid, acetic acid, nitrilotriacetic acid, 2-hydroxyethylethylenediaminetriacetic acid, diethylenetriaminepentaacetic acid, tartaric acid, aluminum dihydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, ethylenediaminetetrapropionic acid, sodium molybdate, gallic acid, tannic acid, boric acid or polyacrylic acid; The auxiliary material includes any one of aluminum oxide, zinc oxide, magnesium oxide, calcium oxide, hydroxyapatite, magnesium hydroxide, zinc hydroxide, hydrophilic silicon dioxide, hydrophobic silicon dioxide, titanium dioxide, iron oxide or aluminum tripolyphosphate, or a combination of at least two thereof; Preferably, the mass ratio of the main material to the auxiliary material is (1-4):

1.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that Based on the mass of the soft magnetic powder being 100 g, the amount of the auxiliary insulating agent used is 0.1 to 0.5 g; Preferably, the auxiliary insulating agent includes any one or a combination of at least two of sodium silicate, silica sol, high base sodium sulfonate, boric acid amine, sodium benzoate, alkylphenol polyoxyethylene ether, fatty acid amide, alkyl alcohol amide, polyoxyethylene nonionic surfactant or polyoxyethylene amide.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that Based on the mass of the soft magnetic powder being 100 g, the amount of the solvent A is 10 to 20 g; Preferably, the solvent A comprises any one of ethanol, xylene, acetone, ethyl acetate, propylene glycol, glycerol, deionized water, propanol or butanol, or a combination of at least two thereof.

6. The preparation method according to any one of claims 1 to 5, It is characterized in that The premixing temperature in step (1) is 40 to 95° C. and the premixing time is 5 to 60 min. Preferably, the mixing temperature in step (1) is 40 to 95° C. and the mixing time is 5 to 60 min; Preferably, the drying temperature in step (1) is 80 to 250° C. and the drying time is 30 to 180 min.

7. The preparation method according to any one of claims 1 to 6, It is characterized in that Based on the mass of the soft magnetic powder being 100 g, the amount of the resin used is 1 to 3.5 g; Preferably, the resin includes any one of epoxy resin, silicone resin, phenolic resin, urea-formaldehyde resin, ketone-alcohol resin, acrylic resin or polyimide resin, or a combination of at least two thereof; Preferably, based on 100 g of the soft magnetic powder, the amount of the solvent B is 10 to 20 g; Preferably, the solvent B includes any one of ethanol, xylene, acetone, ethyl acetate, propylene glycol, glycerol, deionized water, propanol or butanol, or a combination of at least two thereof.

8. An insulating coated soft magnetic powder, It is characterized in that The insulating coated soft magnetic powder is prepared by the preparation method according to any one of claims 1 to 7.

9. An integrated inductor, It is characterized in that The one-piece molded inductor is obtained by pressing the insulating coated soft magnetic powder as claimed in claim 8.

10. Use of the insulating coated soft magnetic powder according to claim 8 or the integrally formed inductor according to claim 9 in electronic components.

Citation Information

Cited By

  • High-frequency low-loss magnetic powder core and preparation method thereof

    CN119943519A

  • Magnetic powder core and preparation method thereof

    CN120432294A