Heat-conducting silver paste, preparation method and application thereof, and connection method of silicon carbide chip and substrate
By using thermally conductive silver paste of sheet silver powder, graphite powder and other components of specific ratios and particle sizes, the problems of excessive internal stress and low thermal conductivity in the pressure sintering process are solved, and silicon carbide chips and substrates are realized Excellent thermal conductivity and low internal stress of the connection.
Patent Information
- Application Number
- CN202411015281.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
In the pressure sintering process, traditional thermal silver paste causes excessive internal stress when connecting silicon carbide chips and substrates, and the thermal conductivity decreases when adding metal or non-metal particles to buffer internal stress.
Thermal silver paste containing a specific proportion and particle size of sheet silver powder, sheet graphite powder, oxygen-containing solvent, adhesive and dispersant is prepared by uniform mixing and three-roll grinding, and the particle size D50 of the sheet silver powder is controlled to be 0.1 to 10 μm, the particle size D10 of sheet graphite powder is 5 μm or more, D50 is 10 to 20 μm, and D90 is 25 μm or less. In combination with the use of oxygen-containing solvents and adhesives, internal stress is reduced and thermal conductivity is improved.
The effect of low internal stress and good thermal conductivity when connecting the silicon carbide chip and the substrate in the pressure sintering process is achieved, and the problems of excessive internal stress and low thermal conductivity in traditional methods are avoided.
Smart Images

Figure BDA0004965512490000101 
Figure BDA0004965512490000111
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new energy, and specifically relates to a thermally conductive silver paste, a preparation method and application thereof, and a method for connecting a silicon carbide chip and a substrate. Background Art
[0002] In recent years, with the widespread popularity of lithium battery new energy vehicles, major OEMs around the world have accelerated the research and application of silicon carbide chips and launched models equipped with 800V silicon carbide IGBT chips on the market. As a typical representative of the third-generation semiconductor materials, silicon carbide has the characteristics of wide bandgap and high thermal conductivity. It is an ideal semiconductor material for high temperature, high voltage, high frequency and high power applications. Silicon carbide power devices can significantly increase the power of electronic equipment and reduce energy consumption, thereby effectively improving the user experience of electric vehicles.
[0003] At present, there are two main types of connection technologies for silicon carbide chips and substrates: one is the traditional leaded or lead-free soldering technology, which uses the reflow process to melt the solder to weld the silicon carbide chip and the substrate together; the other is the pressure sintering process that has emerged in recent years. The pressure sintering process generally uses a thermally conductive metal paste (such as thermally conductive silver paste, thermally conductive copper paste, etc.) with metal powder as the main material. The thermally conductive metal paste is first printed on the substrate, and then silicon carbide is pre-attached to the substrate under heating conditions. Finally, it is placed in a sintering device and subjected to high temperature and high pressure, so that the metal particles in the thermally conductive paste reach the melting point and sinter, thereby connecting the silicon carbide chip and the substrate together. The pressure sintering process connects the silicon carbide chip and the substrate together through high-temperature sintering, but because the sintering process is carried out under high temperature and high pressure, the volume shrinkage caused by sintering will cause stress to accumulate in the sintering layer. This internal stress will increase the probability of failure of the connection between the silicon carbide chip and the substrate, which will seriously affect the reliability of the chip. Although the sintered silver paste made of pure silver powder has low porosity, high density and high thermal conductivity after sintering, it will cause great internal stress due to the shrinkage and close accumulation of silver particles after sintering. This internal stress will cause the connection interface of the IGBT module to be damaged during reliability tests such as hot and cold cycles, thus causing the IGBT module to fail.
[0004] In order to reduce the internal stress generated by the sintering of silver paste, the existing method is to add metal or non-metal particles to the silver paste formula, where the metal particles can be, for example, tungsten powder, molybdenum powder, nickel powder, etc., and the non-metal particles can be, for example, silicon powder, silicon oxide powder, etc. Such additives can effectively buffer the internal stress, but they can also bring negative effects. The most typical negative effect is that since the thermal conductivity of the additive is much smaller than that of pure silver, the thermal conductivity of the sintered layer will be significantly weakened. Summary of the invention
[0005] The first purpose of the present invention is to overcome the defect of excessive internal stress when the silicon carbide chip and the substrate are connected together by the traditional thermal conductive silver paste through the pressure sintering process, and the defect of low thermal conductivity when the silicon carbide chip and the substrate are connected together by the thermal conductive silver paste with added metal or non-metallic particles through the pressure sintering process, and to provide a new thermal conductive silver paste. When the silicon carbide chip and the substrate are connected together by the pressure sintering process, the resulting sintered layer has the advantages of small internal stress and good thermal conductivity.
[0006] The thermally conductive silver paste provided by the present invention contains flaky silver powder, flaky graphite powder, oxygen-containing solvent, adhesive and dispersant in a mass ratio of 100:(0.3-4.5):(5-40):(0.1-1.5):(0.1-1.5); the particle size D50 of the flaky silver powder is 0.1-10 μm; the particle size D10 of the flaky graphite powder is greater than 5 μm, the particle size D50 is 10-20 μm, and the particle size D90 is less than 25 μm.
[0007] In a preferred embodiment, the content of the flaky silver powder is 70 to 90 parts by weight, the content of the flaky graphite powder is 0.3 to 3 parts by weight, the content of the oxygen-containing solvent is 5 to 25 parts by weight, the content of the adhesive is 0.1 to 1 part by weight, and the content of the dispersant is 0.1 to 1 part by weight.
[0008] In a preferred embodiment, the flaky graphite powder is flaky graphite powder.
[0009] In a preferred embodiment, the flash point of the oxygen-containing solvent is 70-150°C.
[0010] In a preferred embodiment, the oxygen-containing solvent is selected from at least one of an ester solvent, an alcohol solvent, an alcohol ether solvent and an organic acid solvent.
[0011] In a preferred embodiment, the adhesive is selected from at least one of thermoplastic polyurethane, thermoplastic rubber and oil-soluble cellulose.
[0012] In a preferred embodiment, the dispersant is selected from at least one of an acrylic dispersant, a polyurethane dispersant and a phosphate dispersant.
[0013] The second object of the present invention is to provide a method for preparing the above-mentioned thermally conductive silver paste, which comprises uniformly mixing flaky silver powder, flaky graphite powder, an oxygen-containing solvent, an adhesive and a dispersant.
[0014] In a preferred embodiment, the mixing method includes dissolving the adhesive in an oxygen-containing solvent, and then adding a dispersant, flaky silver powder and flaky graphite powder to the obtained solution in sequence and continuing to stir and mix evenly, and then grinding the obtained silver paste premix using a three-roll grinder to obtain a thermally conductive silver paste composition.
[0015] The third object of the present invention is to provide the use of the above-mentioned thermally conductive silver paste as an adhesive for silicon carbide power devices.
[0016] The fourth object of the present invention is to provide a method for connecting a silicon carbide chip and a substrate, the method comprising printing the above-mentioned thermal conductive silver paste on the substrate, and then pre-attaching the silicon carbide chip to the surface of the substrate on the side printed with the thermal conductive silver paste, and then sintering at a high temperature to allow the flaky silver powder in the thermal conductive silver paste to reach the melting point, and then connecting the silicon carbide chip and the substrate together.
[0017] The key to the present invention is to use flaky silver powder, flaky graphite powder, oxygen-containing solvent, adhesive and dispersant in specific amounts, and control the particle size D50 of the flaky silver powder to be 0.1-10 μm, while controlling the particle size D10 of the flaky graphite powder to be above 5 μm, the particle size D50 to be 10-20 μm, and the particle size D90 to be below 25 μm. When the heat-conductive silver paste obtained in this way is used to connect the silicon carbide chip and the substrate together through a pressure sintering process, the obtained sintered layer can reduce the internal stress on the basis of obtaining excellent thermal conductivity. The reason may be that: on the one hand, the carbon atoms in the flake graphite powder are a single-layer structure, and the oxygen-containing solvent can be effectively inserted between the layers of the flake graphite powder, making the interlayer bonding force very low. The flake graphite powder is used to modify the flake silver powder, which can effectively reduce the modulus of the silver powder after sintering. The reduction of the modulus is conducive to the reduction of internal stress. In addition, the particle size D10 of the flake graphite powder is controlled to be above 5μm, the particle size D50 is controlled to be controlled to be 10-20μm, and the particle size D90 is controlled to be below 25μm. It can effectively reduce the shrinkage of silver powder after sintering and increase the bulk density of sintered silver powder, which is also beneficial to reduce internal stress. That is, the synergistic effect of modulus, volume shrinkage and bulk density can effectively reduce the internal stress of sintered silver paste. On the other hand, the thermal conductivity of flaky graphite powder is above 1000W / m·K, which is much larger than the thermal conductivity of other metals such as tungsten, molybdenum, nickel and non-metals such as silicon, which can make up for the problem of weakened thermal conductivity of the sintered layer due to the use of additives. DETAILED DESCRIPTION
[0018] The "range" disclosed in the present invention is defined in the form of a lower limit and / or an upper limit, and a given range is defined by selecting a lower limit and / or an upper limit. The range defined in this way can be inclusive or exclusive of the end value, and can be combined in any way, that is, any lower limit can be combined with any upper limit to form an undefined range, and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value itself can be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an undefined range.
[0019] The thermally conductive silver paste provided by the present invention contains flaky silver powder, flaky graphite powder, oxygen-containing solvent, adhesive and dispersant. The mass ratio of the flaky silver powder, flaky graphite powder, oxygen-containing solvent, adhesive and dispersant is 100:(0.3-4.5):(5-40):(0.1-1.5):(0.1-1.5). Taking the total content of flaky silver powder as 100 parts by weight, the content of flaky graphite powder is 0.3-4.5 parts by weight, such as 0.3, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 parts by weight or any value therebetween; the content of oxygen-containing solvent is 5-40 parts by weight, such as 5, 10, 15, 20, 25, 30, 35, 40 parts by weight or any value therebetween; the content of adhesive is 0.1-1.5 parts by weight, such as 0.1, 0.3, 0.5, 0.8, 1, 1.2, 1.5 parts by weight or any value therebetween; the content of dispersant is 0.1-1.5 parts by weight, such as 0.1, 0.3, 0.5, 0.8, 1, 1.2, 1.5 parts by weight or any value therebetween. The content of each component in the thermal conductive silver paste can be any point value within the above range, which is not enumerated here. In a preferred embodiment, the content of the flaky silver powder is 70 to 90 parts by weight, the content of the flaky graphite powder is 0.3 to 3 parts by weight, the content of the oxygen-containing solvent is 5 to 25 parts by weight, the content of the adhesive is 0.1 to 1 part by weight, and the content of the dispersant is 0.1 to 1 part by weight. At this time, the components can play a better synergistic role, which is more conducive to the elimination of internal stress and the improvement of thermal conductivity.
[0020] In the present invention, the particle size D50 of the flaky silver powder is 0.1 to 10 μm, such as 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm or any value therebetween. The particle size D50 of the flaky silver powder can be any point value within the above range, which is not enumerated here. The term "flaky silver powder" refers to pure silver powder that is in the form of thin flakes in a microscopic state. The particle size of flaky silver powder has a crucial influence on the sintering temperature. When the particle size is too small, the sintering temperature will be greatly reduced, which will cause the thermal conductive silver paste to sinter prematurely during drying and pre-lamination, thereby reducing the adhesion of the silver paste to the chip and reducing the thermal conductivity. When the particle size is too large, the sintering temperature is too high, which will cause the thermal conductive silver paste to be unable to achieve effective sintering at the sintering temperature, and will also lead to an increase in internal stress.
[0021] In the present invention, the particle size D10 of the flake graphite powder is 5 μm or more, such as 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 14.5 μm, 15 μm, 15.5 μm, 16 μm, 16.5 μm, 17 μm, 17.5 μm, 18 μm or any value therebetween; the particle size D50 is 10 to 20 μm, such as 10 μm, 10.5 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 14.5 μm, 15 μm, 15.5 μm, 16 μm, 16.5 μm, 17 μm, 17.5 μm, 18 μm or any value therebetween; , 11μm, 11.5μm, 12μm, 12.5μm, 13μm, 13.5μm, 14μm, 14.5μm, 15μm, 15.5μm, 16μm, 16.5μm, 17μm, 17.5μm, 18μm, 18.5μm, 19μm, 19.5μm, 20μm or any value therebetween; particle size D90 is less than 25μm, such as 25μm, 24.5μm, 24μm, 23.5μm, 23μm, 22.5μm, 22μm, 21.5μm, 21μm, 20.5μm, 20μm or any value therebetween. The values of particle size D10, D50 and D90 of flake graphite powder can be any point value within the above range, which are not enumerated here. When the particle size D10 of the flaky graphite powder is less than 5 μm and / or the particle size D50 is less than 10 μm, not only can the internal stress generated by sintering not be effectively reduced, but the thermal conductivity after sintering tends to decrease; when the particle size D50 of the flaky graphite powder is greater than 20 μm and / or the particle size D90 is greater than 25 μm, the printability of the thermal conductive silver paste deteriorates, and the adhesion after sintering tends to decrease.
[0022] In the present invention, the flake graphite powder is preferably flaky graphite powder. The flaky graphite powder not only has a single-layer carbon atom structure with low interlayer bonding force, but also has a large specific surface area, which can effectively reduce the internal stress of the silver paste after high-temperature sintering and give it better thermal conductivity. The flaky graphite powder can be purchased commercially or prepared according to various existing methods.
[0023] In the present invention, the term "oxygen-containing solvent" refers to an inert liquid solvent including oxygen atoms in the molecule. The flash point of the oxygen-containing solvent is preferably 70 to 150°C, such as 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C or any value therebetween. When the flash point of the oxygen-containing solvent is lower than 70°C, it may cause voids and pores in the thermal conductive silver paste during sintering; when the flash point of the oxygen-containing solvent is higher than 150°C, it will affect the drying speed of the thermal conductive silver paste. Specific examples of oxygen-containing solvents include, but are not limited to, at least one of ester solvents, alcohol solvents, alcohol ether solvents and organic acid solvents. Among them, the ester solvent can be, for example, at least one of ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, dimethyl adipate, diethyl adipate, dibutyl adipate, diethylene glycol monoethyl ether acetate and divalent acid ester (DBE). The alcohol solvent can be, for example, at least one of lauryl alcohol, isodecyl alcohol, 2-octyl-1-dodecanol, 2-ethyl-1,3-hexanediol, tridecanol, pine alcohol and cyclohexanol. The alcohol ether solvent can be, for example, at least one of ethylene glycol dibutyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether and triethylene glycol dimethyl ether. The organic acid solvent can be, for example, at least one of 2-methylbutyric acid, hexanoic acid, heptanoic acid, octanoic acid, 2-ethylbutyric acid and 2-ethylhexanoic acid. Most preferably, the oxygen-containing solvent is selected from at least one of pine alcohol, diethylene glycol butyl ether acetate and ethylene glycol dibutyl ether.
[0024] In the present invention, the purpose of adding the adhesive is to provide a certain adhesive force during pre-lamination, so that the chip can be temporarily fixed on the dried thermal conductive silver paste to facilitate the subsequent sintering. The adhesive can be any existing organic compound with high temperature viscosity, for example, it can be selected from at least one of thermoplastic polyurethane, thermoplastic rubber, and oil-soluble cellulose.
[0025] In the present invention, the purpose of adding the dispersant is to achieve a uniform and stable mixing effect of the flaky silver powder and the flaky graphite powder. The dispersant can be specifically selected from at least one of an acrylic dispersant, a polyurethane dispersant and a phosphate dispersant.
[0026] The second object of the present invention is to provide a method for preparing the above-mentioned thermally conductive silver paste, which comprises mixing flaky silver powder, flaky graphite powder, oxygen-containing solvent, adhesive and dispersant. Wherein, the mixing method can be carried out in various existing ways, for example, the above components can be added at one time and mixed evenly, or several of them can be mixed evenly in any order, and then the remaining materials are added and mixed evenly. In a preferred embodiment, the mixing method includes dissolving the adhesive in an oxygen-containing solvent, and then adding a dispersant, flaky silver powder and flaky graphite powder to the obtained solute in turn and continuing to stir and mix evenly, and then grinding the obtained silver paste premix with a three-roll grinder to obtain a thermally conductive silver paste composition. Wherein, the dissolution temperature is preferably 45 to 55°C, such as 45°C, 48°C, 50°C, 52°C, 55°C or any value therebetween.
[0027] The third object of the present invention is to provide the use of the above-mentioned thermally conductive silver paste as an adhesive for silicon carbide power devices.
[0028] The fourth object of the present invention is to provide a method for connecting a silicon carbide chip and a substrate, the method comprising printing the above-mentioned thermal conductive silver paste on a substrate, and then pre-pasting the silicon carbide chip on the side surface of the substrate printed with the thermal conductive silver paste, and then sintering at high temperature to make the flaky silver powder in the thermal conductive silver paste reach the melting point and then connecting the silicon carbide chip and the substrate together. Among them, the pre-pasting method is generally to place the silicon carbide chip on the side surface of the substrate printed with the thermal conductive silver paste and keep it at a certain temperature and pressure for a certain time, wherein the temperature can be 110-130°C, such as 110°C, 115°C, 120°C, 125°C, 130°C or any value therebetween; the pressure can be 0.3-1MPa, such as 0.3MPa, 0.5MPa, 0.8MPa, 1MPa or any value therebetween; the time can be 1-10s, such as 1s, 3s, 5s, 8s, 10s or any value therebetween. The conditions for high temperature sintering generally include a temperature of 240 to 260°C, such as 240°C, 245°C, 250°C, 255°C, 260°C or any value therebetween; a pressure of 10 to 30MPa, such as 10MPa, 12MPa, 15MPa, 18MPa, 20MPa, 22MPa, 25MPa, 28MPa, 30MPa or any value therebetween; and a time of 1 to 5min, such as 1min, 2min, 3min, 4min, 5min or any value therebetween.
[0029] The present invention will be described in detail below by way of examples. The examples of the embodiments are intended to explain the present invention and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0030] In the following examples and comparative examples, the sources of the raw materials are as follows:
[0031] Thermoplastic polyurethane adhesive was purchased from Lubrizol Corporation, brand number 58125;
[0032] Thermoplastic rubber adhesive was purchased from Baling Petrochemical Company, brand name YH-792E;
[0033] The oil-soluble cellulose binder was purchased from Yuemei Chemical Company and the brand name was cellulose ethyl ether (EC);
[0034] The phosphate dispersant was purchased from BYK Chemical Company with the brand name W9010;
[0035] The acrylic dispersant was purchased from BYK Chemical Company, with the brand name BYK3550;
[0036] The polyurethane dispersant was purchased from BYK Chemical Company, with the brand name BYK163;
[0037] Terpineol was purchased from Yatai United Chemical Company, the grade was analytically pure terpineol, and the flash point was 98°C;
[0038] Diethylene glycol butyl ether acetate was purchased from Aladdin, with a flash point of 105°C;
[0039] Ethylene glycol dibutyl ether was purchased from Aladdin, with a flash point of 85°C;
[0040] n-Tetradecane was purchased from Aladdin and had a flash point of 100°C.
[0041] In the following examples and comparative examples, the shapes of the flaky silver powder and the flaky graphite are measured using a scanning electron microscope (SEM), and the particle sizes of the flaky silver powder and the flaky graphite are measured using a laser particle size distribution analyzer.
[0042] Examples 1-7
[0043] The adhesive is dissolved in an oxygen-containing solvent at 50° C. under stirring conditions, and then a dispersant, flaky silver powder and flaky graphite powder are added to the obtained solution in sequence and stirred and mixed evenly, and then the obtained silver paste premix is ground using a three-roll grinder to obtain a thermally conductive silver paste. The types and contents of the components in the thermally conductive silver paste are shown in Table 1.
[0044] Comparative Example 1
[0045] A thermally conductive silver paste was prepared according to the method of Example 4, except that the amount of flaky graphite powder was adjusted to 0.1 parts by weight, and the other conditions were the same as those of Example 4 to obtain a reference thermally conductive silver paste. The types and contents of the components in the reference thermally conductive silver paste are shown in Table 1.
[0046] Comparative Example 2
[0047] A thermally conductive silver paste was prepared according to the method of Example 4, except that the flake silver powder with a particle size D50 of 1 μm was replaced with a flake silver powder with a particle size D50 of 0.05 μm, and the other conditions were the same as those of Example 4 to obtain a reference thermally conductive silver paste. The types and contents of the components in the reference thermally conductive silver paste are shown in Table 1.
[0048] Comparative Example 3
[0049] A thermally conductive silver paste was prepared according to the method of Example 4, except that the flaky graphite powder (D50=12 μm, D10=6 μm and D90=23 μm) was replaced by the same weight of flaky graphite powder (D50=3 μm and D10=0.4 μm), and the other conditions were the same as those of Example 4 to obtain a reference thermally conductive silver paste. The types and contents of the components in the reference thermally conductive silver paste are shown in Table 1.
[0050] Comparative Example 4
[0051] A thermally conductive silver paste was prepared according to the method of Example 4, except that the flaky graphite powder (D50=12 μm, D10=6 μm and D90=23 μm) was replaced by the same weight of flaky graphite powder (D50=38 μm and D90=150 μm), and the other conditions were the same as those of Example 4 to obtain a reference thermally conductive silver paste. The types and contents of the components in the reference thermally conductive silver paste are shown in Table 1.
[0052] Comparative Example 5
[0053] A thermally conductive silver paste was prepared according to the method of Example 4, except that pineneol was replaced by the same weight portion of non-oxygenated solvent n-tetradecane, and the other conditions were the same as those of Example 4 to obtain a reference thermally conductive silver paste. The types and contents of the components in the reference thermally conductive silver paste are shown in Table 1.
[0054] Test Case
[0055] (1) Adhesion test: The thermal conductive silver paste obtained in the above embodiments and the reference thermal conductive silver paste obtained in the comparative examples were uniformly printed on the silver-plated surface of the silver-plated ceramic substrate using a printer, with a printing thickness of 80 μm and a size of 6×6 mm. The thermal conductive silver paste was then placed in an oven at 130°C for 30 minutes and taken out after being completely dried. The silver-plated ceramic substrate was then placed on a laminating machine, and a 5×5 mm SiC chip was pre-laminated on the dried silver paste. The pre-lamination process was to apply a pressure of 0.5 MPa to the SiC chip at 120°C and maintain it for 4 seconds. The pre-laminated sample was sintered at 250°C and 20 MPa for 3 minutes using a sintering machine. The sintered sample was tested for shear force using a push knife tester (DAGE4000). The results are shown in Table 1.
[0056] (2) Internal stress test: The internal stress of the thermal conductive silver paste is determined by testing its storage modulus after sintering. In general, the larger the storage modulus, the greater the internal stress; conversely, the smaller the internal stress. Storage modulus test method: Use a printer to evenly print the thermal conductive silver paste obtained in the above embodiments and the reference thermal conductive silver paste obtained in each comparative example on a glass plate, with a printing thickness of 150 μm and a size of 5×60 mm. Then place it in an oven at 130°C and dry for 60 minutes. After the thermal conductive silver paste is completely dried, take it out. The dried sample is sintered in a sintering machine at 250°C and 20 MPa for 3 minutes. Since the silver paste cannot be sintered onto the glass plate, the sintered sample can be easily removed from the glass plate. The storage modulus of the sintered silver paste sheet was tested using DMA. The results are shown in Table 1.
[0057] (3) Thermal conductivity test: The thermally conductive silver paste obtained in the above embodiments and the reference thermally conductive silver paste obtained in the comparative examples were poured into a mold with a diameter of 12.7 mm and a depth of 2 mm, and the surface was flattened with a scraper. Then, the thermally conductive silver paste was placed in an oven at 130°C for 4 hours and taken out after it was completely dried. The dried thermally conductive silver paste sample was placed in a sintering machine and sintered at 250°C and 20 MPa for 3 minutes. The thermal conductivity of the silver paste sample was tested by the laser flash method. The results are shown in Table 1.
[0058]
[0059] Table 2
[0060]
[0061] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A thermally conductive silver paste, characterized in that: The thermally conductive silver paste contains flaky silver powder, flaky graphite powder, oxygen-containing solvent, adhesive and dispersant in a mass ratio of 100:(0.3-4.5):(5-40):(0.1-1.5):(0.1-1.5); the particle size D50 of the flaky silver powder is 0.1-10 μm; the particle size D10 of the flaky graphite powder is greater than 5 μm, the particle size D50 is 10-20 μm, and the particle size D90 is less than 25 μm.
2. The thermally conductive silver paste according to claim 1, characterized in that: The content of the flaky silver powder is 70 to 90 parts by weight, the content of the flaky graphite powder is 0.3 to 3 parts by weight, the content of the oxygen-containing solvent is 5 to 25 parts by weight, the content of the adhesive is 0.1 to 1 part by weight, and the content of the dispersant is 0.1 to 1 part by weight.
3. The thermally conductive silver paste according to claim 1 or 2, characterized in that: The flaky graphite powder is flaky graphite powder.
4. The thermally conductive silver paste according to claim 1 or 2, characterized in that: The flash point of the oxygen-containing solvent is 70-150° C.; preferably, the oxygen-containing solvent is selected from at least one of ester solvents, alcohol solvents, alcohol ether solvents and organic acid solvents.
5. The thermally conductive silver paste according to claim 1 or 2, characterized in that: The adhesive is selected from at least one of thermoplastic polyurethane, thermoplastic rubber and oil-soluble cellulose.
6. The thermally conductive silver paste according to claim 1 or 2, characterized in that: The dispersant is selected from at least one of an acrylic dispersant, a polyurethane dispersant and a phosphate dispersant.
7. The method for preparing the thermally conductive silver paste according to any one of claims 1 to 6, characterized in that: The method comprises uniformly mixing flaky silver powder, flaky graphite powder, an oxygen-containing solvent, a binder and a dispersant.
8. The method for preparing the thermally conductive silver paste according to claim 7, characterized in that: The mixing method includes dissolving the adhesive in an oxygen-containing solvent, adding a dispersant, flaky silver powder and flaky graphite powder to the obtained solution in sequence and continuing to stir and mix them evenly, and then grinding the obtained silver paste premix using a three-roll grinder to obtain a thermally conductive silver paste composition.
9. Use of the thermally conductive silver paste according to any one of claims 1 to 6 as an adhesive for silicon carbide power devices.
10. A method for connecting a silicon carbide chip and a substrate, characterized in that: The method comprises printing the thermal conductive silver paste described in any one of claims 1 to 6 on a substrate, pre-attaching a silicon carbide chip to the surface of the substrate on the side printed with the thermal conductive silver paste, and then sintering at a high temperature so that the flaky silver powder in the thermal conductive silver paste reaches the melting point, and then connecting the silicon carbide chip and the substrate together.