Planar photoconductive switch and manufacturing method thereof
By introducing a conductive region or conductive layer inside the planar photoconductive switch, the breakdown problem caused by current concentration is solved, the withstand voltage performance and service life of the device are improved, and the on-resistance is reduced.
Patent Information
- Application Number
- CN202411422144.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-10-12
AI Technical Summary
Existing planar photoconductive switches have current concentration at the electrode edges in the dark state, leading to breakdown and reduced lifespan, as well as high on-resistance.
By introducing conductive areas or conductive layers inside planar photoconductive switches, current is transported from the surface to the interior, forming a conductive channel, alleviating current concentration, and reducing on-resistance.
It effectively improves the voltage withstand performance and lifespan of the device, while significantly increasing the photocurrent and reducing the on-resistance.
Smart Images

Figure CN118919584A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor structures, and in particular relates to a planar photoconductive switch and a manufacturing method thereof. Background Art
[0002] Gallium nitride (GaN), as one of the leaders of third-generation semiconductors, has many excellent physical and chemical properties, such as a bandgap of 3.4 eV, a critical breakdown field of 3.3 MV / cm, a saturated electron migration velocity of 2.5×107 cm / s, a direct bandgap structure, and resistance to strong acids and alkalis. These properties ensure its broad application prospects in high-frequency, high-power, optoelectronic devices, and other fields.
[0003] Iron-doped semi-insulating gallium nitride (SI-GaN:Fe), a type of gallium nitride, has been widely studied because it can be used both as an isolation layer between devices to improve breakdown characteristics and as a substrate for devices. Furthermore, due to its excellent performance in both the light state (low on-resistance), dark state (low leakage current), and light-dark state transitions (short carrier lifetime), it is considered the most promising semiconductor material for high-frequency, high-power photoconductive switching.
[0004] Photoconductive semiconductor switches (PCSS) are semiconductor switches triggered by a specific excitation light source. They offer advantages such as small size, low loss, high output power, fast response speed, and high repetition rate. They have broad application prospects in fields such as medicine and aerospace. Photoconductive switching devices can be broadly categorized into vertical and planar types.
[0005] Among these devices, the electrodes of planar photoconductive switches are fabricated on the same side of the substrate (usually the Ga side). This makes them popular due to their simple fabrication and low device cost. However, since the electrodes are on the same side of the substrate, the current concentrates at the electrode edges in the dark state, making the switch susceptible to breakdown and significantly reducing the device's lifespan. The conduction characteristics of planar photoconductive switches are closely related to the surface dislocation density and crystal quality of the substrate material, making them more susceptible to surface flashover under high voltage. Furthermore, the photocurrent in the on-state of planar devices is too low, and the on-resistance is high.
[0006] The information disclosed in this background technology section is only intended to enhance understanding of the overall background of the invention and should not be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the Invention
[0007] The purpose of the present invention is to provide a planar photoconductive switch and a method for manufacturing the same, which can convert current from surface transport to current transport within the body, effectively alleviate the current concentration phenomenon at the edge of the electrode, improve the voltage resistance and service life of the device, and at the same time, significantly increase the photocurrent and reduce the on-resistance.
[0008] In order to achieve the above object, a specific embodiment of the present invention provides the following technical solutions: A planar photoconductive switch, comprising: A substrate having a first doping source, the substrate having a first surface, a conductive region formed in the substrate that is not doped or has a second doping source, wherein the resistance of the conductive region is smaller than the resistance of the substrate; an epitaxial layer having a third doping source, formed on the first surface and covering the conductive region, wherein a resistance of the epitaxial layer is greater than a resistance of the conductive region; a first electrode formed on the epitaxial layer; a second electrode formed on the epitaxial layer and spaced apart from the first electrode; In the thickness direction of the substrate, the projection of the conductive area partially overlaps with the projection of the first electrode and the projection of the second electrode.
[0009] In one or more embodiments of the present invention, the substrate material includes GaN single crystal, the first doping source includes Fe, and the doping concentration is 1×10 18 cm -3 -1×10 19 cm -3 .
[0010] In one or more embodiments of the present invention, the substrate material includes GaN single crystal, the conductive region has a second doping source, and the second doping source includes Si and Ge with a doping concentration of 5×10 17 cm -3 -1×10 19 cm -3 .
[0011] In one or more embodiments of the present invention, the material of the epitaxial layer includes GaN single crystal, and the third doping source includes Fe with a doping concentration of 1×10 18 cm -3 -1×10 19 cm -3 .
[0012] In one or more embodiments of the present invention, the resistivity of the substrate is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the substrate is 1×108 cm -3 -1×10 9 cm -3 .
[0013] In one or more embodiments of the present invention, the thickness of the conductive region is in the range of 20 μm to 100 μm.
[0014] In one or more embodiments of the present invention, the resistivity of the epitaxial layer is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the epitaxial layer is 1×10 8 cm -3 -1×10 9 cm -3 .
[0015] In one or more embodiments of the present invention, the epitaxial layer has a thickness ranging from 5 μm to 50 μm.
[0016] In one or more embodiments of the present invention, the first electrode includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence on the epitaxial layer, the thickness of the first Ti layer is in the range of 5nm-30nm, the thickness of the Al layer is in the range of 80nm-130nm, the thickness of the second Ti layer is in the range of 50nm-100nm, and the thickness of the Au layer is in the range of 50nm-150nm.
[0017] In one or more embodiments of the present invention, edge corners of the first electrode are configured to be arc-shaped.
[0018] In one or more embodiments of the present invention, the second electrode includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence on the epitaxial layer, the thickness of the first Ti layer is in the range of 5nm-30nm, the thickness of the Al layer is in the range of 80nm-130nm, the thickness of the second Ti layer is in the range of 50nm-100nm, and the thickness of the Au layer is in the range of 50nm-150nm.
[0019] In one or more embodiments of the present invention, edge corners of the second electrode are configured to be arc-shaped.
[0020] A method for manufacturing a planar light-conductive switch, comprising: providing a conductive structure having a second doping source or being undoped; forming an epitaxial structure having a first doping source and / or a third doping source around the conductive structure, wherein the resistance of the epitaxial structure is greater than the resistance of the conductive structure; forming a first electrode and a second electrode spaced apart from each other on the same surface of the epitaxial structure, wherein, in a direction perpendicular to the first electrode and / or the second electrode, a projection of the first electrode and a projection of the second electrode both partially overlap with a projection of the conductive structure; A method for manufacturing a planar light-conductive switch, comprising: Providing a substrate having a first doping source, wherein the substrate has a first surface; forming a conductive region having a second doping source or being non-doped on the first surface, wherein the resistance of the conductive region is lower than the resistance of the substrate; forming an epitaxial layer on the first surface, which covers the conductive region and has a third doping source, wherein the resistance of the epitaxial layer is greater than the resistance of the conductive region; A first electrode and a second electrode spaced apart from each other are formed on the epitaxial layer.
[0021] A planar photoconductive switch, comprising: a substrate having a first dopant source, the substrate having a first surface; a non-doped conductive layer or a conductive layer having a second doping source, formed on the first surface of the substrate, wherein the resistance of the conductive layer is lower than the resistance of the substrate; an epitaxial layer having a third doping source, formed on the conductive layer, wherein a resistance of the epitaxial layer is greater than a resistance of the conductive layer; a first electrode formed on the epitaxial layer; The second electrode is formed on the epitaxial layer and spaced apart from the first electrode.
[0022] In one or more embodiments of the present invention, the substrate material includes GaN single crystal, the first doping source includes Fe, and the doping concentration is 1×10 18 cm -3 -1×10 19 cm -3 .
[0023] In one or more embodiments of the present invention, the conductive layer comprises a GaN single crystal, and the conductive layer has a second doping source, wherein the second doping source comprises Si and Ge, and the doping concentration is 5×10 17 cm -3 -1×10 19 cm -3 .
[0024] In one or more embodiments of the present invention, the material of the epitaxial layer includes GaN single crystal, and the third doping source includes Fe with a doping concentration of 1×10 18 cm -3 -1×10 19 cm-3 .
[0025] In one or more embodiments of the present invention, the resistivity of the substrate is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the substrate is 1×10 8 cm -3 -1×10 9 cm -3 .
[0026] In one or more embodiments of the present invention, the thickness of the conductive layer is in the range of 20 μm to 100 μm.
[0027] In one or more embodiments of the present invention, the resistivity of the epitaxial layer is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the epitaxial layer is 1×10 8 cm -3 -1×10 9 cm -3 .
[0028] The thickness of the epitaxial layer is in the range of 5 μm to 50 μm.
[0029] In one or more embodiments of the present invention, the first electrode includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence on the epitaxial layer, the thickness of the first Ti layer is in the range of 5nm-30nm, the thickness of the Al layer is in the range of 80nm-130nm, the thickness of the second Ti layer is in the range of 50nm-100nm, and the thickness of the Au layer is in the range of 50nm-150nm.
[0030] In one or more embodiments of the present invention, edge corners of the first electrode are configured to be arc-shaped.
[0031] In one or more embodiments of the present invention, the second electrode includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence on the epitaxial layer, the thickness of the first Ti layer is in the range of 5nm-30nm, the thickness of the Al layer is in the range of 80nm-130nm, the thickness of the second Ti layer is in the range of 50nm-100nm, and the thickness of the Au layer is in the range of 50nm-150nm.
[0032] In one or more embodiments of the present invention, edge corners of the second electrode are configured to be arc-shaped.
[0033] A method for manufacturing a planar light-conductive switch, comprising: Providing a substrate having a first doping source, wherein the substrate has a first surface; forming a non-doped conductive layer or a conductive layer having a second doping source on the first surface, wherein the resistance of the conductive layer is lower than the resistance of the substrate; forming an epitaxial layer having a third doping source on the conductive layer, wherein the resistance of the epitaxial layer is greater than the resistance of the conductive layer; A first electrode and a second electrode spaced apart from each other are formed on the epitaxial layer.
[0034] Compared with the prior art, the planar photoconductive switch and its manufacturing method of the present invention can transform the current from surface transport to internal transport by introducing an internal conductive area or conductive layer, which can effectively alleviate the current concentration phenomenon at the edge of the electrode and improve the voltage resistance and service life of the device. At the same time, the introduction of the conductive area or conductive layer can significantly increase the photocurrent and reduce the on-resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0036] Figure 1 Schematic diagram of the structure of the planar photoconductive switch in Example 1 of the present invention; Figure 2 1 is a top view of the structure of the planar light-conductive switch in Example 1 of the present invention; Figure 3 Flow chart of the manufacturing process of the planar photoconductive switch in Example 1 of the present invention; Figure 4 is another process flow chart for manufacturing the planar photoconductive switch in Example 1 of the present invention; Figure 5 Schematic diagram of the structure of a planar photoconductive switch in Example 2 of the present invention; Figure 6 2 is a top view of the structure of a planar light-conductive switch in Example 2 of the present invention; Figure 7 Flow chart of the manufacturing process of the planar photoconductive switch in Example 2 of the present invention; Figure 8a This is a simulation diagram of the dark-state internal current of an existing planar photoconductive switch; Figure 8b This is a simulation diagram of the dark-state internal current of the planar photoconductive switch of the present invention; Figure 9This is a comparison diagram of the on-state photocurrent simulation of the planar photoconductive switch of the present invention and the existing planar photoconductive switch. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts should fall within the scope of protection of the present invention.
[0038] As mentioned in the background technology, when the existing planar photoconductive switch is in the dark state, the current is mainly transported through the surface and concentrated at the edge of the electrode, which can easily lead to surface flashover discharge, causing the electrode edge to be broken down, affecting the device's voltage resistance and service life.
[0039] Based on this, the present invention provides a planar photoconductive switch and a method for fabricating it. By introducing a relatively low-resistance conductive region or layer within the planar photoconductive switch, current is shifted from surface transport to bulk transport. This effectively alleviates current concentration at the electrode edges, significantly reducing the occurrence of surface flashover discharge and improving the withstand voltage and service life of the planar photoconductive switch. Furthermore, in the on-state, the photocurrent of the planar photoconductive switch with the conductive region or layer is significantly greater than that of the switch without it, indicating that the introduction of the conductive region or layer reduces the on-resistance.
[0040] refer to Figure 1 and Figure 2 As shown, Embodiment 1 of the present invention provides a planar photoconductive switch, comprising a substrate 10 having a first doping source, a conductive region 20 that is undoped or has a second doping source, an epitaxial layer 30 having a third doping source, and a first electrode 40 and a second electrode 50. The conductive region 20 is formed within the substrate 10, and the resistance of the conductive region 20 is lower than that of the substrate 10. The epitaxial layer 30 is formed on the surface of the substrate 10 and covers the conductive region 20, and the resistance of the epitaxial layer 30 is higher than that of the conductive region 20. The first electrode 40 and the second electrode 50 are formed on the surface of the epitaxial layer 30, and are spaced apart from each other. The first electrode 40 and the second electrode 50 are positioned such that, in the thickness direction of the substrate 10, the projection of the conductive region 20 partially overlaps with the projection of the first electrode 40 and the projection of the second electrode 50.
[0041] The substrate 10 has a first surface 10a. The material of the substrate 10 is GaN single crystal, the first doping source is Fe, and the doping concentration of Fe is in the range of 1×10 18 cm -3-1×10 19 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 The substrate 10, except for the conductive region 20, has a first doping source Fe in all other regions. After Fe doping, the substrate 10 exhibits a high resistance state, thereby making the substrate 10 semi-insulating and having a high resistance. The resistivity range of the substrate 10 at room temperature (300 K) is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, the carrier concentration range is 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 The size of the substrate 10 is preferably 10 mm×10 mm.
[0042] The conductive region 20 is formed in the middle region of the first surface 10a of the substrate 10 and extends deep into the substrate 10. The conductive region 20 has a second doping source or is undoped. When the conductive region 20 has a second doping source, the second doping source includes Si and Ge, and the doping concentration is 5×10 17 cm -3 -1×10 19 cm -3 After Si or Ge doping, the resistance of the conductive region 20 decreases significantly, so that the conductive region 20 has a lower resistance than the substrate 10 , thereby forming a conductive channel between the first electrode 40 and the second electrode 50 .
[0043] It can be understood that when the conductive region 20 is undoped, since other regions of the substrate 10 are Fe-doped, the resistance of the undoped conductive region 20 is still lower than that of the other Fe-doped regions.
[0044] The thickness of the conductive region 20 is smaller than that of the substrate 10. The thickness of the conductive region 20 ranges from 20 μm to 100 μm.
[0045] The epitaxial layer 30 is formed on the first surface 10a of the substrate 10 and completely covers the conductive region 20. The epitaxial layer 30 is also made of GaN single crystal, and the third doping source is Fe, with a doping concentration range of 1×10 18 cm -3 -1×10 19 cm -3, preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 , which is the same as the doping concentration of the substrate 10. Similarly, after Fe doping, the epitaxial layer 30 presents a high resistance state like the substrate 10, making the epitaxial layer 30 also have semi-insulating properties and high resistance. As a result, the entire device forms a low resistance region at the location of the conductive region 20, forming a conductive channel that is easier to transmit current. The resistivity range of the epitaxial layer 30 at room temperature (300 K) is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, the carrier concentration range is 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 The thickness of the epitaxial layer 30 is in the range of 5 μm to 50 μm.
[0046] The first electrode 40 is formed on the epitaxial layer 30. The first electrode 40 includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence. The thickness of the first Ti layer ranges from 5 nm to 30 nm, preferably 20 nm. The thickness of the Al layer ranges from 80 nm to 130 nm, preferably 130 nm. The thickness of the second Ti layer ranges from 50 nm to 100 nm, preferably 50 nm. The thickness of the Au layer ranges from 50 nm to 150 nm, preferably 150 nm.
[0047] The second electrode 50 is formed on the epitaxial layer 30. The second electrode 50 includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence. The thickness of the first Ti layer ranges from 5 nm to 30 nm, preferably 20 nm. The thickness of the Al layer ranges from 80 nm to 130 nm, preferably 130 nm. The thickness of the second Ti layer ranges from 50 nm to 100 nm, preferably 50 nm. The thickness of the Au layer ranges from 50 nm to 150 nm, preferably 150 nm.
[0048] In the above technical solution, by introducing the conductive region 20 inside the device to form a conductive channel, the current is converted from surface transport to body transport, which can effectively alleviate the current concentration phenomenon at the electrode edge and reduce the on-resistance.
[0049] In order to further effectively alleviate the electric field concentration and prevent the first electrode 40 and the second electrode 50 from being broken down, the edge corners of the first electrode 40 and the second electrode 50 are both configured to be arc-shaped.
[0050] Exemplarily, the first electrode 40 and the second electrode 50 are arranged in a rounded rectangle shape, the rounded rectangle is 7 mm long and 3 mm wide, and the first electrode 40 and the second electrode 50 are spaced 1 mm apart.
[0051] refer to Figure 3 As shown, the present invention also provides a method for manufacturing the above-mentioned planar light-conductive switch, which specifically includes the following steps: S1, providing a conductive structure having a second doping source or a non-doped conductive structure.
[0052] S2, forming an epitaxial structure having a first doping source and / or a third doping source on a peripheral surface of the conductive structure, wherein a resistance of the epitaxial structure is greater than a resistance of the conductive structure.
[0053] S3, forming a first electrode and a second electrode spaced apart on the same surface of the epitaxial structure, wherein in a direction perpendicular to the first electrode and / or the second electrode, a projection of the first electrode and a projection of the second electrode partially overlap with a projection of the conductive structure.
[0054] Wherein, in step S1, when the conductive structure has a second doping source, a conductive layer having the second doping source can be directly grown by HVPE epitaxy first, and then the surrounding areas of the conductive layer can be etched to form the desired conductive structure, and the conductive structure can be used as a conductive region in a subsequent device, or the surrounding areas of the conductive layer can be not etched and the conductive region can be directly used as a conductive region in a subsequent device. Alternatively, an undoped conductive layer can be directly grown by HVPE epitaxy first, and then the second doping source can be doped in the conductive layer by ion implantation or other methods, and finally the undoped area of the conductive layer can be etched to form the desired conductive structure. When the conductive structure is undoped, a conductive layer can be directly grown by epitaxy, and the surrounding areas of the conductive layer can be etched to form the desired conductive structure, or the surrounding areas of the conductive layer can be not etched and the conductive region can be directly used as a conductive region in a subsequent device.
[0055] The conductive structure is made of GaN, and the second doping source is Si or Ge, with a doping concentration range of 5×10 17 cm -3 -1×10 19 cm -3 , the thickness of the conductive structure ranges from 20μm to 100μm.
[0056] In step S2, an epitaxial structure having the first doping source and / or the third doping source can be grown directly on each peripheral surface of the conductive structure by HVPE epitaxy, wherein the epitaxial structure includes a substrate having the first doping source and an epitaxial layer having the third doping source, and the epitaxial structure completely covers the conductive structure. Alternatively, an undoped epitaxial structure can be grown directly on each peripheral surface of the conductive structure by HVPE epitaxy, and then the epitaxial structure is doped with the first doping source and / or the third doping source by ion implantation or other methods.
[0057] The epitaxial structure is made of GaN, the first doping source and the third doping source are both Fe, and the doping concentration range is 1×10 18 cm -3 -1×10 19 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 , the resistivity range of the epitaxial structure is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, and the carrier concentration of the epitaxial structure ranges from 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 .
[0058] refer to Figure 4 As shown, the present invention also provides another method for manufacturing the above-mentioned planar light-conductive switch, which specifically includes the following steps: S10, providing a substrate having a first doping source, wherein the substrate has a first surface.
[0059] S20, forming a conductive region having a second doping source or a non-doped region on the first surface, wherein the resistance of the conductive region is smaller than the resistance of the substrate; S30 , forming an epitaxial layer covering the conductive region and having a third doping source on the first surface, wherein the resistance of the epitaxial layer is greater than the resistance of the conductive region.
[0060] S40 , forming a first electrode and a second electrode spaced apart from each other on the epitaxial layer.
[0061] In step S10, a substrate with the first doping source may be directly grown by HVPE epitaxy, or an undoped substrate may be directly grown by HVPE epitaxy and then doped with the first doping source by ion implantation or other methods.
[0062] The substrate material is GaN, the first doping source is Fe, and the doping concentration range is 1×10 18 cm -3 -1×10 19 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 , the substrate resistivity range is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, and the substrate carrier concentration range is 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 .
[0063] In step S20, when the conductive structure has a second doping source, a conductive structure having the second doping source can be directly grown in the central region of the first surface of the substrate by HVPE epitaxy, with the edge of the conductive structure exposing the first surface of the substrate. The conductive structure serves as a conductive region in a subsequent device. Alternatively, a conductive layer having the second doping source is directly grown on the first surface of the substrate, and then the surrounding area of the conductive layer is etched to form a conductive structure located in the central region of the first surface of the substrate. Alternatively, an undoped conductive structure can be directly grown by HVPE epitaxy, with the edge of the conductive structure exposing the first surface of the substrate, and then the conductive structure is doped with the second doping source by ion implantation or the like. Alternatively, an undoped conductive layer can be directly grown by HVPE epitaxy, and then a portion of the conductive layer is doped with the second doping source by ion implantation or the like, and finally the undoped region of the conductive layer is etched to form a conductive structure. Alternatively, the second doping source can be directly doped into the substrate from the central region on the first surface of the substrate by ion implantation or the like to form a conductive region. When the conductive structure is undoped, a conductive layer can be directly grown in the central area of the first surface of the substrate by epitaxy, or in step S1, when the substrate is ion-implanted with a first doping source, a mask is used to retain an undoped area in the substrate to form a conductive area.
[0064] The material of the conductive structure (conductive area) is GaN, the second doping source is Si and Ge, and the doping concentration range is 5×10 17 cm -3 -1×10 19 cm -3 The thickness of the conductive structure (conductive area) ranges from 20 μm to 100 μm.
[0065] In step S30, an epitaxial layer having the third dopant source can be grown directly on the first surface of the substrate by HVPE epitaxy, with the epitaxial layer completely covering the conductive structure. Alternatively, an undoped epitaxial layer can be grown directly on the first surface of the substrate by HVPE epitaxy, and then the epitaxial layer can be doped with the first dopant source by ion implantation or other methods.
[0066] The epitaxial layer material is GaN, the third doping source is Fe, and the doping concentration range is 1×10 18 cm -3 -1×10 19 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 , the resistivity range of the epitaxial layer is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, the carrier concentration of the epitaxial layer is in the range of 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 .
[0067] refer to Figure 5 and Figure 6 As shown, Embodiment 2 of the present invention provides a planar photoconductive switch, comprising a substrate 10 having a first dopant source, a conductive layer 200 that is undoped or has a second dopant source, an epitaxial layer 30 having a third dopant source, a first electrode 40, and a second electrode 50. The conductive layer 200 is formed on the surface of the substrate 10, and the resistance of the conductive layer 200 is lower than that of the substrate 10. The epitaxial layer 30 is formed on the surface of the conductive layer 200, and the resistance of the epitaxial layer 30 is higher than that of the conductive layer 200. The first electrode 40 and the second electrode 50 are formed on the surface of the epitaxial layer 30, and the first electrode 40 and the second electrode 50 are spaced apart.
[0068] The substrate 10 has a first surface 10a. The material of the substrate 10 is GaN single crystal, the first doping source is Fe, and the doping concentration of Fe is in the range of 1×10 18 cm -3 -1×10 19 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 After Fe doping, the substrate 10 exhibits a high resistance state, which makes the substrate 10 semi-insulating and has a high resistance. The resistivity range of the substrate 10 at room temperature (300 K) is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, the carrier concentration range is 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 The size of the substrate 10 is preferably 10 mm×10 mm.
[0069] The conductive layer 200 is formed on the first surface 10a of the substrate 10. The conductive layer 200 has a second doping source or is undoped. When the conductive layer 200 has a second doping source, the second doping source includes Si and Ge, and the doping concentration is 5×10 17 cm -3 -1×10 19 cm -3 After Si or Ge doping, the resistance of the conductive layer 200 decreases significantly, so that the conductive layer 200 has a lower resistance than the substrate 10 , thereby forming a conductive channel between the first electrode 40 and the second electrode 50 .
[0070] It can be understood that when the conductive layer 200 is undoped, since the substrate 10 is Fe-doped, the resistance of the undoped conductive layer 200 is still lower than the resistance of the Fe-doped substrate 10 .
[0071] The thickness of the conductive layer 200 is smaller than that of the substrate 10. The thickness of the conductive layer 200 is in the range of 20 μm to 100 μm.
[0072] The epitaxial layer 30 is formed on the conductive layer 200. The epitaxial layer 30 is also made of GaN single crystal, and the third doping source is Fe, with a doping concentration range of 1×10 18 cm -3 -1×1019 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 , which is the same as the doping concentration of the substrate 10. Similarly, after Fe doping, the epitaxial layer 30 presents a high resistance state like the substrate 10, making the epitaxial layer 30 also semi-insulating and having a high resistance. As a result, the entire device forms a low resistance in the conductive layer 200, constructing a conductive channel that is easier to transmit current. The resistivity range of the epitaxial layer 30 at room temperature (300 K) is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, the carrier concentration range is 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 The thickness of the epitaxial layer 30 is in the range of 5 μm to 50 μm.
[0073] The first electrode 40 is formed on the epitaxial layer 30. The first electrode 40 includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence. The thickness of the first Ti layer ranges from 5 nm to 30 nm, preferably 20 nm. The thickness of the Al layer ranges from 80 nm to 130 nm, preferably 130 nm. The thickness of the second Ti layer ranges from 50 nm to 100 nm, preferably 50 nm. The thickness of the Au layer ranges from 50 nm to 150 nm, preferably 150 nm.
[0074] The second electrode 50 is formed on the epitaxial layer 30. The second electrode 50 includes a first Ti layer, an Al layer, a second Ti layer, and an Au layer stacked in sequence. The thickness of the first Ti layer ranges from 5 nm to 30 nm, preferably 20 nm. The thickness of the Al layer ranges from 80 nm to 130 nm, preferably 130 nm. The thickness of the second Ti layer ranges from 50 nm to 100 nm, preferably 50 nm. The thickness of the Au layer ranges from 50 nm to 150 nm, preferably 150 nm.
[0075] In the above technical solution, by introducing a conductive layer 200 into the interior of the device to form a conductive channel, the current is converted from surface transport to body transport, which can effectively alleviate the current concentration phenomenon at the electrode edge and reduce the on-resistance.
[0076] In order to further effectively alleviate the electric field concentration and prevent the first electrode 40 and the second electrode 50 from being broken down, the edge corners of the first electrode 40 and the second electrode 50 are both configured to be arc-shaped.
[0077] Exemplarily, the first electrode 40 and the second electrode 50 are arranged in a rounded rectangle shape, the rounded rectangle is 7 mm long and 3 mm wide, and the first electrode 40 and the second electrode 50 are spaced 1 mm apart.
[0078] refer to Figure 7 As shown, the present invention also provides another method for manufacturing the above-mentioned planar light-conductive switch, which specifically includes the following steps: S100 , providing a substrate having a first doping source, wherein the substrate has a first surface.
[0079] S200, forming a non-doped conductive layer or a conductive layer having a second doping source on the first surface, wherein the resistance of the conductive layer is less than the resistance of the substrate; S300, forming an epitaxial layer having a third doping source on the conductive layer, wherein the resistance of the epitaxial layer is greater than the resistance of the conductive layer; S400 , forming a first electrode and a second electrode spaced apart from each other on the epitaxial layer.
[0080] In step S100, a substrate with the first doping source may be directly grown by HVPE epitaxy, or an undoped substrate may be directly grown by HVPE epitaxy and then doped with the first doping source by ion implantation or other methods.
[0081] The substrate material is GaN, the first doping source is Fe, and the doping concentration range is 1×10 18 cm -3 -1×10 19 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 , the substrate resistivity range is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, and the substrate carrier concentration range is 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 .
[0082] In step S200, when the conductive layer has a second dopant source, the conductive layer having the second dopant source can be directly grown on the first surface of the substrate by HVPE epitaxy. Alternatively, an undoped conductive layer can be directly grown by HVPE epitaxy and then doped with the second dopant source by ion implantation or other methods. If the conductive layer is undoped, the conductive layer can be directly grown on the first surface of the substrate by epitaxy.
[0083] The conductive layer is made of GaN, and the second doping source is Si or Ge, with a doping concentration range of 5×10 17 cm -3 -1×10 19 cm -3 The thickness of the conductive layer ranges from 20 μm to 100 μm.
[0084] In step S300, an epitaxial layer having the third dopant source may be grown directly on the conductive layer by HVPE epitaxy. Alternatively, an undoped epitaxial layer may be grown directly on the conductive layer by HVPE epitaxy, and then the epitaxial layer may be doped with the first dopant source by ion implantation or other methods.
[0085] The epitaxial layer material is GaN, the third doping source is Fe, and the doping concentration range is 1×10 18 cm -3 -1×10 19 cm -3 , preferably 2×10 18 cm -3 -5×10 18 cm -3 , for example 5×10 18 cm -3 , the resistivity range of the epitaxial layer is 1×10 8 Ω·cm-1×10 9 Ω·cm, preferably 1×10 8 Ω·cm, the carrier concentration of the epitaxial layer is in the range of 1×10 8 cm -3 -1×10 9 cm -3 , preferably 6.2×10 8 cm -3 .
[0086] Figure 8a This is a simulation diagram of the dark state internal current of an existing planar photoconductive switch. Figure 8b This is a simulation diagram of the dark state internal current of the planar photoconductive switch of the present invention, wherein the horizontal axis is the device length and the vertical axis is the device height, both in micrometers. Figure 8a and Figure 8bBy comparison, it can be seen that in the existing planar photoconductive switch without a conductive area or conductive layer, the current is mainly concentrated at the edge of the electrode, while in the planar photoconductive switch of the present invention that introduces a conductive area or conductive layer (conductive channel), the current is mainly concentrated inside the device, and the current is transformed from surface transport to internal transport.
[0087] Figure 9 This is a comparison diagram of the on-state photocurrent simulation of the planar photoconductive switch of the present invention and the existing planar photoconductive switch. Figure 9 It can be seen that after the conductive area or conductive layer (conductive channel) is introduced into the planar photoconductive switch of the present invention, the photocurrent peak value increases significantly, which means that the introduction of the conductive area or conductive layer (conductive channel) can significantly reduce the on-resistance.
[0088] Compared with the prior art, the planar photoconductive switch and its manufacturing method of the present invention can transform the current from surface transport to internal transport by introducing an internal conductive area or conductive layer, which can effectively alleviate the current concentration phenomenon at the edge of the electrode and improve the voltage resistance and service life of the device. At the same time, the introduction of the conductive area or conductive layer can significantly increase the photocurrent and reduce the on-resistance.
[0089] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the invention can be embodied in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as illustrative and non-restrictive, and the scope of the invention is defined by the appended claims, not the foregoing description, and all variations within the meaning and range of equivalents of the claims are intended to be included therein. Any reference sign in a claim should not be construed as limiting the claim to which it relates.
[0090] In addition, it should be understood that although this specification is described in terms of implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
Claims
1. A planar photoconductive switch, It is characterized in that include: A substrate having a first doping source, the substrate having a first surface, a non-doped conductive region or a conductive region having a second doping source formed in the substrate, and a resistance of the conductive region being smaller than a resistance of the substrate; an epitaxial layer having a third doping source, formed on the first surface and covering the conductive region, wherein a resistance of the epitaxial layer is greater than a resistance of the conductive region; A first electrode formed on the epitaxial layer; A second electrode is formed on the epitaxial layer and spaced apart from the first electrode; Wherein, in the thickness direction of the substrate, the projection of the conductive area partially overlaps with the projection of the first electrode and the projection of the second electrode.
2. The planar photoconductive switch according to claim 1, It is characterized in that The material of the substrate includes GaN single crystal, and the first doping source includes Fe with a doping concentration of 1×10 18 cm -3 -1×10 19 cm -3 and / or, The material of the substrate includes GaN single crystal, the conductive region has a second doping source, and the second doping source includes Si and Ge, with a doping concentration of 5×10 17 cm -3 -1×10 19 cm -3 and / or, The material of the epitaxial layer includes GaN single crystal, and the third doping source includes Fe with a doping concentration of 1×10 18 cm -3 -1×10 19 cm -3 .
3. The planar photoconductive switch according to claim 1, It is characterized in that The resistivity of the substrate is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the substrate is 1×10 8 cm -3 -1×10 9 cm -3 and / or, The thickness of the conductive area is in the range of 20 μm to 100 μm; and / or, The resistivity of the epitaxial layer is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the epitaxial layer is 1×10 8 cm -3 -1×10 9 cm -3 and / or, The thickness of the epitaxial layer is in the range of 5 μm to 50 μm.
4. The planar photoconductive switch according to claim 1, It is characterized in that The first electrode comprises a first Ti layer, an Al layer, a second Ti layer, and an Au layer which are sequentially stacked on the epitaxial layer, the first Ti layer has a thickness range of 5nm-30nm, the Al layer has a thickness range of 80nm-130nm, the second Ti layer has a thickness range of 50nm-100nm, and the Au layer has a thickness range of 50nm-150nm; and / or, The edge corner of the first electrode is configured to be arc-shaped; and / or, The second electrode comprises a first Ti layer, an Al layer, a second Ti layer, and an Au layer which are sequentially stacked on the epitaxial layer, wherein the thickness of the first Ti layer is in the range of 5nm-30nm, the thickness of the Al layer is in the range of 80nm-130nm, the thickness of the second Ti layer is in the range of 50nm-100nm, and the thickness of the Au layer is in the range of 50nm-150nm; and / or, The edge corner of the second electrode is configured to be arc-shaped.
5. A method for manufacturing a planar photoconductive switch, It is characterized in that include: providing a conductive structure having a second doping source or being undoped; forming an epitaxial structure having a first doping source and / or a third doping source around the conductive structure, wherein the resistance of the epitaxial structure is greater than the resistance of the conductive structure; forming a first electrode and a second electrode spaced apart from each other on the same surface of the epitaxial structure, wherein in a direction perpendicular to the first electrode and / or the second electrode, a projection of the first electrode and a projection of the second electrode both partially overlap with a projection of the conductive structure; or, Providing a substrate having a first doping source, the substrate having a first surface; forming a conductive region having a second doping source or being non-doped on the first surface, wherein the resistance of the conductive region is lower than the resistance of the substrate; forming an epitaxial layer covering the conductive region and having a third doping source on the first surface, wherein the resistance of the epitaxial layer is greater than the resistance of the conductive region; A first electrode and a second electrode spaced apart from each other are formed on the epitaxial layer.
6. A planar photoconductive switch, It is characterized in that include: A substrate having a first doping source, the substrate having a first surface; a non-doped conductive layer or a conductive layer having a second doping source, formed on the first surface of the substrate, wherein the resistance of the conductive layer is lower than the resistance of the substrate; an epitaxial layer having a third doping source, formed on the conductive layer, wherein the resistance of the epitaxial layer is greater than the resistance of the conductive layer; A first electrode formed on the epitaxial layer; The second electrode is formed on the epitaxial layer and spaced apart from the first electrode.
7. The planar photoconductive switch according to claim 6, It is characterized in that The material of the substrate includes GaN single crystal, and the first doping source includes Fe with a doping concentration of 1×10 18 cm -3 -1×10 19 cm -3 and / or, The conductive layer is made of GaN single crystal, and the conductive layer has a second doping source, which includes Si and Ge, with a doping concentration of 5×10 17 cm -3 -1×10 19 cm -3 and / or, The material of the epitaxial layer includes GaN single crystal, and the third doping source includes Fe with a doping concentration of 1×10 18 cm -3 -1×10 19 cm -3 .
8. The planar photoconductive switch according to claim 6, It is characterized in that The resistivity of the substrate is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the substrate is 1×10 8 cm -3 -1×10 9 cm -3 and / or, The thickness of the conductive layer is in the range of 20 μm to 100 μm; and / or, The resistivity of the epitaxial layer is in the range of 1×10 8 Ω·cm-1×10 9 Ω·cm, the carrier concentration range of the epitaxial layer is 1×10 8 cm -3 -1×10 9 cm -3 and / or, The thickness of the epitaxial layer is in the range of 5 μm to 50 μm.
9. The planar photoconductive switch according to claim 6, It is characterized in that The first electrode comprises a first Ti layer, an Al layer, a second Ti layer, and an Au layer which are sequentially stacked on the epitaxial layer, the first Ti layer has a thickness range of 5nm-30nm, the Al layer has a thickness range of 80nm-130nm, the second Ti layer has a thickness range of 50nm-100nm, and the Au layer has a thickness range of 50nm-150nm; and / or, The edge corner of the first electrode is configured to be arc-shaped; and / or, The second electrode comprises a first Ti layer, an Al layer, a second Ti layer, and an Au layer which are sequentially stacked on the epitaxial layer, wherein the thickness of the first Ti layer is in the range of 5nm-30nm, the thickness of the Al layer is in the range of 80nm-130nm, the thickness of the second Ti layer is in the range of 50nm-100nm, and the thickness of the Au layer is in the range of 50nm-150nm; and / or, The edge corner of the second electrode is configured to be arc-shaped.
10. A method for manufacturing a planar photoconductive switch, It is characterized in that include: Providing a substrate having a first doping source, the substrate having a first surface; forming a non-doped conductive layer or a conductive layer having a second doping source on the first surface, wherein the resistance of the conductive layer is lower than the resistance of the substrate; forming an epitaxial layer having a third doping source on the conductive layer, wherein the resistance of the epitaxial layer is greater than the resistance of the conductive layer; A first electrode and a second electrode spaced apart from each other are formed on the epitaxial layer.
Citation Information
Patent Citations
Photoconductive semiconductor switch structure
CN102945887A
Method for using proton irradiation to prepare ultrafast response GaN photoconductive switch
CN107369736A
Photoconductive switch and preparation method thereof
CN108735849A
Photoconductive switch and preparation method thereof
CN118448503A
Photoconductive semiconductor switch laterally fabricated alongside GAN on si field-effect transistors
TW202243128A
Cited By
Magnetic response composite electrode structure for photoconductive semiconductor switch and method of tuning thereof
CN122766105A