Ga2O3 ultraviolet detector and preparation method and application thereof
High-quality Ga2O3 films were prepared by atomic layer deposition and annealed. Combined with photolithography and magnetron sputtering technology, the problem of low light-dark current ratio and low responsiveness of Ga2O3 ultraviolet photodetector is solved, and faster spectrum Response speed and wider range of high-frequency detection applications.
Patent Information
- Application Number
- CN202410847720.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the Ga2O3 film produced by the PVD method of physical vapor deposition is poor in crystal quality, resulting in the problem of small light-dark current ratio and low responsiveness.
Atomic layer deposition method is used to prepare amorphous Ga2O3 film on the substrate and annealed in a nitrogen atmosphere. Then, the interfinger electrode is prepared by using photolithography, magnetron sputtering technology and peeling technology to improve the Ga2O3 ultraviolet photodetector Crystallization mass and spectral response speed.
By improving the crystallization quality of Ga2O3 film, the spectral response speed of the gallium oxide-based ultraviolet photodetector is enhanced, making it more widely used in the field of high-frequency signal detection.
Smart Images

Figure CN118919600A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of development of photoelectric detection materials for ultraviolet light signal detection, and relates to a Ga2O3-based ultraviolet photoelectric detector and a preparation method and application thereof. Background Art
[0002] Solar-blind ultraviolet detectors are widely used in missile tracking, ozone hole monitoring, optical communications, biological and chemical analysis, environmental monitoring and other fields due to their advantages such as low background noise, high security and high anti-interference ability.
[0003] Gallium oxide is a deep ultraviolet transparent ultra-wide bandgap semiconductor material. Compared with traditional wide bandgap semiconductors, Ga2O3 has a wider bandgap width (~4.9eV), ultra-high breakdown electric field, excellent thermal stability and chemical stability, and its bandgap directly corresponds to the deep ultraviolet band, so it has broad application prospects in high temperature, high frequency, high power electronic devices and solar-blind ultraviolet detectors. High-quality gallium oxide films are prepared by atomic layer deposition, thereby improving the responsiveness and light-to-dark current ratio of gallium oxide-based ultraviolet photodetector devices. Gallium oxide ultraviolet photodetectors prepared by physical vapor deposition (PVD) have problems such as small light-to-dark current ratio, low light response, and slow spectral response speed. Summary of the invention
[0004] In order to address the problems existing in the prior art, the present invention provides a Ga2O3-based ultraviolet photodetector and a preparation method and application thereof, thereby solving the technical problems of a small light-to-dark current ratio and low responsiveness caused by the poor crystallization quality of the Ga2O3 thin film prepared by the physical vapor deposition (PVD) method in the prior art.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for preparing a Ga2O3 ultraviolet photodetector comprises the following steps:
[0007] S1: an amorphous Ga2O3 film is prepared on a substrate by atomic layer deposition, and the product is annealed in a nitrogen atmosphere to obtain a crystalline Ga2O3 film;
[0008] S2: preparing interdigital electrodes on the crystallized Ga2O3 film by using photolithography, magnetron sputtering technology and stripping process to obtain the Ga2O3 ultraviolet detector.
[0009] Preferably, in step S1, in the process of preparing the amorphous Ga2O3 thin film on the substrate by atomic layer deposition, trimethylgallium is used as the Ga source, O3 with a purity of 99.99% is used as the O source, and during the deposition process, nitrogen with a purity of 99.9995% is used as the carrier gas.
[0010] Preferably, in step S1, before preparing the amorphous Ga2O3 thin film on the substrate by atomic layer deposition, the pressure of the reaction chamber is controlled to be 0.3-0.5 Pa and the temperature of the substrate is controlled to be 200-300°C.
[0011] Preferably, in step S1, when an amorphous Ga2O3 thin film is prepared on a substrate by atomic layer deposition, a Ga source precursor and an O source precursor are cyclically intermittently injected; the injection time of the Ga source precursor in one cycle is 0.3 to 0.7 s, and the injection time of the O source precursor is 0.3 to 0.7 s. After the injection is completed, nitrogen is used for purging before entering the next cycle.
[0012] Preferably, the nitrogen purge time is 6 to 9 seconds.
[0013] Preferably, the number of cycles is 1200-2400.
[0014] Preferably, the thickness of the amorphous Ga2O3 film is 50 to 110 nm.
[0015] Preferably, during the annealing process, the annealing temperature is 700-1000° C. and the annealing time is 1-2 hours.
[0016] A Ga2O3 ultraviolet photoelectric detector is prepared by the above method.
[0017] The above-mentioned Ga2O3 ultraviolet photodetector is used in high-frequency signal detection.
[0018] Compared with the prior art, the present invention has the following beneficial technical effects:
[0019] The present invention discloses a method for preparing a Ga2O3 ultraviolet photodetector, comprising the following steps: preparing an amorphous Ga2O3 film on a substrate by an atomic layer deposition method, annealing the product in a nitrogen atmosphere to obtain a crystallized Ga2O3 film; preparing interdigitated electrodes on the crystallized Ga2O3 film by using a photolithography process, a magnetron sputtering technology and a stripping process to obtain the Ga2O3 ultraviolet detector. The method adopts an atomic layer deposition method to prepare a Ga2O3 film. The gallium oxide film prepared by the method has high crystal quality, is more uniform and dense, has fewer internal defects, and is more conducive to reducing the capture and release of photogenerated carriers by internal defects of the film, thereby preparing a gallium oxide-based ultraviolet photodetector with a faster spectral response speed, so that the detector can be used in a higher frequency detection field.
[0020] Furthermore, in step S1, in the process of preparing the amorphous Ga2O3 thin film on the substrate by atomic layer deposition, trimethylgallium is used as the Ga source, and O3 with a purity of 99.99% is used as the O source. During the deposition process, nitrogen with a purity of 99.9995% is used as the carrier gas, which can carry the Ga source and the O source to the surface area of the substrate.
[0021] Furthermore, in step S1, before preparing the amorphous Ga2O3 film on the substrate by atomic layer deposition, the pressure of the reaction chamber is controlled to be 0.3-0.5 Pa and the temperature of the substrate is controlled to be 200°C-300°C, so that the reaction precursor can react normally in the reaction chamber.
[0022] Furthermore, in step S1, when an amorphous Ga2O3 thin film is prepared on a substrate by atomic layer deposition, a Ga source precursor and an O source precursor are cyclically intermittently injected; the injection time of the Ga source precursor in one cycle is 0.3 to 0.7 s, and the injection time of the O source precursor is 0.3 to 0.7 s. After the injection is completed, nitrogen is purged, and then the next cycle is entered, so that the Ga source and O source reaction precursors can be delivered into the reaction chamber.
[0023] Furthermore, the nitrogen purge time is 6s to 9s, so as to clean the reaction chamber and remove the reaction by-products.
[0024] Furthermore, the number of cycles is 1200 to 2400, so that Ga2O3 films with different thickness requirements can be obtained in the entire growth deposition process.
[0025] Furthermore, the thickness of the amorphous Ga2O3 film is 50-110 nm, so that detectors with active layers of different thicknesses can be obtained.
[0026] Furthermore, during the annealing process, the annealing temperature is 700-1000° C. and the annealing time is 1-2 hours, which can improve the crystallization quality of the thin film. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 It is a schematic diagram of a process for preparing a Ga2O3 ultraviolet detector in the present invention;
[0029] Figure 2X-ray diffraction patterns of Ga2O3 thin films at different annealing temperatures in the present invention;
[0030] Figure 3 This is a diagram of the film cross-section test results in the present invention;
[0031] Figure 4 AFM images of Ga2O3 thin films at different annealing temperatures in the present invention;
[0032] Figure 5 The surface roughness test results of Ga2O3 thin films at different annealing temperatures in the present invention;
[0033] Figure 6 The test results of the film transmission spectrum at different annealing temperatures in the present invention;
[0034] Figure 7 The relationship curve between the optical band gap of Ga2O3 film and the annealing temperature in the present invention;
[0035] Figure 8 The IV characteristics of the detector at different annealing temperatures in the present invention;
[0036] Fig. 9 The effect of annealing temperature on (a) the responsivity and (b) the light-to-dark current ratio of the detector in the present invention;
[0037] Fig.10 The effect of annealing temperature on the spectral response characteristics of the detector in the present invention;
[0038] Fig.11 It is the characteristic curve of the detector responding to 254nm ultraviolet light at different annealing temperatures in the present invention;
[0039] Fig.12 The single-cycle normalized curve of the detector time response at different annealing temperatures in the present invention;
[0040] Fig.13 The IV characteristics of the detectors with different interdigital spacings under 254nm ultraviolet light in the present invention;
[0041] Fig.14 The effect of the interdigital spacing on the light-dark suppression ratio and responsivity of the detector in the present invention;
[0042] Fig.15 The effect of the interdigital spacing on the spectral response characteristics of the detector in the present invention;
[0043] Fig.16 It is the It characteristic curve of the detector responding to 254nm ultraviolet light at different interdigital spacings in the present invention;
[0044] Fig.17It is a single-cycle normalized curve of the detector time response under different interdigital spacings in the present invention. DETAILED DESCRIPTION
[0045] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0046] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0047] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0048] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0049] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0050] As shown in FIG1 , the present invention provides a schematic flow diagram of a method for preparing a Ga2O3 ultraviolet detector. The amorphous Ga2O3 thin film growth device used in the specific experiment is a Beneq TFS200 atomic layer deposition device. The Ga2O3 thin film preparation process is as follows:
[0051] 1. Substrate cleaning: During the experiment, a double-polished c-plane sapphire substrate was used as the substrate. Acetone, deionized water and anhydrous ethanol were used to ultrasonically clean the substrate in turn to remove impurities and oil stains on the substrate surface. Finally, the cleaned substrate was blown dry with a nitrogen gun and dried for standby use to ensure that the substrate surface was clean and dry.
[0052] 2. Thin film deposition: After the substrate is cleaned, the substrate is sent to the reaction chamber of the ALD (TFS-200, Beneq) deposition system. During the reaction process, TMGa (trimethylgallium, cold source) and O3 (99.99%) are used as Ga source and O source respectively, of which O3 is sent to the ALD reaction chamber in the form of natural volatilization under vapor pressure; high-purity nitrogen (99.9995%) is used as the carrier gas in the reaction process to clean the reaction chamber. During the reaction process, the deposition pressure of the reaction chamber is first pumped to 0.3-0.5 Pa, and then the substrate temperature is heated and kept warm for 5 minutes to ensure that the substrate temperature rises to 200-300°C, and then the Ga source and O source reaction precursors are sent to the reaction chamber in turn by opening the corresponding valves. In a complete reaction cycle, the injection time of Ga source precursor into the reaction chamber is 0.3-0.7s, and the injection time of O source precursor is 0.3-0.7s. During this period, N2 purge is required for 6-9s to clean the reaction chamber and remove reaction byproducts. The entire reaction needs to be repeated for 1200-2400 cycles, and the preparation time is about 13h to obtain an amorphous Ga2O3 film with a thickness of about 50-110nm.
[0053] 3. Annealing treatment: In order to crystallize the deposited amorphous Ga2O3 film, reduce internal defects of the film and improve the quality of the film, the prepared amorphous Ga2O3 film is subjected to high-temperature post-annealing treatment, wherein the post-annealing process parameters are: annealing temperature is 700-1000°C, annealing atmosphere is N2, and annealing time is fixed at 1-2h.
[0054] 4. Detector preparation: After the Ga2O3 film is prepared, the MSM-type gallium oxide-based ultraviolet photodetector with interdigitated electrode morphology is prepared by photolithography, magnetron sputtering and lift-off processes.
[0055] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0056] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0057] Example 1
[0058] A method for preparing a Ga2O3 ultraviolet photodetector comprises the following steps:
[0059] 1. Substrate cleaning: During the experiment, a double-polished c-plane sapphire substrate was used as the substrate. Acetone, deionized water and anhydrous ethanol were used to ultrasonically clean the substrate in turn to remove impurities and oil stains on the substrate surface. Finally, the cleaned substrate was blown dry with a nitrogen gun and dried for standby use to ensure that the substrate surface was clean and dry.
[0060] 2. Thin film deposition: After the substrate is cleaned, the substrate is sent to the reaction chamber of the ALD (TFS-200, Beneq) deposition system. During the reaction process, TMGa (trimethylgallium, cold source) and O3 (99.99%) are used as Ga source and O source respectively, of which O3 is sent to the ALD reaction chamber in the form of natural volatilization under vapor pressure; high-purity nitrogen (99.9995%) is used as the carrier gas in the reaction process to clean the reaction chamber. During the reaction process, the deposition pressure of the reaction chamber is first pumped to 0.3Pa, and then the substrate temperature is heated to 300℃ and kept warm for 5min to ensure that the substrate temperature rises to 300℃, and then the Ga source and O source reaction precursors are sent to the reaction chamber in turn by opening the corresponding valves. In a complete reaction cycle, the time for the Ga source precursor to be injected into the reaction chamber is 0.5s, and the time for the O source precursor to be injected into the reaction chamber is 0.7s. During this period, 8s of N2 purge is required to clean the reaction chamber and remove the reaction by-products. The entire reaction needs to be repeated for 2315 cycles, and the preparation time is about 13 hours to obtain an amorphous Ga2O3 film with a thickness of about 103nm. The Beneq TFS200 atomic layer deposition equipment was used in this experiment.
[0061] 3. Annealing treatment: In order to crystallize the deposited amorphous Ga2O3 film, reduce the internal defects of the film and improve the quality of the film, the prepared amorphous Ga2O3 film is subjected to high-temperature post-annealing treatment, wherein the post-annealing process parameters are: annealing temperature is 700°C, annealing atmosphere is N2, and annealing time is fixed at 2h.
[0062] 4. Detector preparation: After the Ga2O3 film is prepared, the MSM-type gallium oxide-based ultraviolet photodetector with interdigitated electrode morphology is prepared by photolithography, magnetron sputtering and lift-off processes.
[0063] Example 2
[0064] The difference from Example 1 is that the annealing temperature is 800°C.
[0065] Example 3
[0066] The difference from Example 1 is that the annealing temperature is 900°C.
[0067] Example 4
[0068] The difference from Example 1 is that the annealing temperature is 1000°C.
[0069] The technical solution of the present invention is described through the following tests and in conjunction with the accompanying drawings:
[0070] In order to study the effect of annealing temperature on the properties of Ga2O3 thin films deposited by ALD method, after the film was prepared, the film performance characterization methods such as XRD test, AFM test, TEM test and UV-Vis test were used to analyze the effect of annealing temperature on the film performance.
[0071] (1) Effect of annealing temperature on the crystal structure of thin films
[0072] Figure 2 The XRD test patterns of Ga2O3 films at different annealing temperatures. The samples prepared at annealing temperatures of 700℃ to 1000℃ all showed diffraction peaks of (-201), (-311) and -603) of polycrystalline β-Ga2O3 at 2θ angles of 18.95°, 38.4° and 59.19° respectively (PDF#43-1012). The sample prepared at 700℃ also showed a diffraction peak of (403) crystal plane of β phase. It can be seen that the sample prepared at 700℃ showed poor crystal quality. As the annealing temperature increased to 900℃, the (403) crystal plane diffraction peak disappeared, and the peak intensity of each diffraction peak of the film gradually increased, showing preferential growth along the β (-201) crystal direction. When the annealing temperature was further increased to 1000℃, the peak intensity of each diffraction peak of the film was significantly weakened. Therefore, the film sample annealed at 900℃ showed the best crystal quality.
[0073] In order to further analyze the effect of annealing temperature on the crystallization quality of the film, the Jade software was used to analyze the half-width of the main diffraction peak β (-201) diffraction peak, and the results are shown in Table 1. It can be seen that when the annealing temperature increases to 800 ° C, the FWHM diffraction peak of the film decreases significantly, indicating that the film defects are reduced and the degree of crystallization is improved after high-temperature annealing. The average grain size of the film is calculated using the Scherrer formula. As the annealing temperature increases from 700 ° C to 1000 ° C, the grain size of the film increases from 25.3nm to 37.7nm. It can be seen that compared with the Ga2O3 film prepared by the magnetron sputtering process, the film sample prepared by the ALD process has better crystallization quality.
[0074] Table 1
[0075]
[0076] (2) Effect of annealing temperature on film micromorphology
[0077] Figure 3The cross-sectional test results of the Ga2O3 film after annealing show that the film thickness is 103.26nm. The surface morphology of the Ga2O3 film was characterized and tested using an atomic force microscope, and the changes in the surface roughness of the film after annealing were analyzed. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that the surface morphology of the film is uniform and dense. Figure 5 It can be seen that the surface roughness of the films with annealing temperatures of 700°C to 1000°C are 1.05nm, 1.28nm, 1.82nm and 1.6nm respectively. It can be seen that the annealing temperature has a great influence on the distribution of the film surface morphology.
[0078] There are discontinuous large-sized island particles on the surface of the sample annealed at 700℃. As the annealing temperature increases to 900℃, the number of surface island grains increases continuously, the uniformity increases, the surface roughness also increases significantly, and the grain boundaries become clearer. This is because high-temperature annealing can induce composite crystallization between adjacent grains in the film, thereby increasing the grain size of the film. When the annealing temperature is further increased to 1000℃, the surface roughness of the film decreases slightly. Compared with the Sn-doped Ga2O3 film prepared by magnetron sputtering, the Ga2O3 film prepared by ALD process has a smoother, more uniform and denser morphology, which is more conducive to the preparation of high-performance gallium oxide-based ultraviolet photodetectors.
[0079] (3) Effect of annealing temperature on the optical properties of thin films
[0080] Figure 6 The transmission spectra of Ga2O3 films at different annealing temperatures show that the film samples annealed at different temperatures have steep absorption edges in the deep ultraviolet band of 200nm to 280nm, and have high transmittance in the visible light region. With the increase of annealing temperature, the transmittance of the film in the visible light region remains basically unchanged, and the optical absorption edge blue-shifts. The blue shift of the optical absorption edge may be due to the transformation of the amorphous film into a β-phase film and the recrystallization of the film grains. At the same time, compared with the Ga2O3 film prepared by magnetron sputtering, the film samples prepared by ALD method show lower ultraviolet transmittance in the deep ultraviolet region, which indicates that the Ga2O3 film prepared by ALD method has better deep ultraviolet absorption and solar-blind ultraviolet detection capabilities than the film prepared by magnetron sputtering process.
[0081] In order to further analyze the effect of annealing temperature on the optical band gap of annealed samples, the optical band gap of samples was calculated by fitting the tested absorption spectrum according to the Tauc formula. The results are shown in Figure 7 As shown, it can be seen that the Eg of Ga2O3 film gradually increases with the increase of annealing temperature.
[0082] In order to analyze the effect of Ga2O3 film annealing temperature on the performance of gallium oxide-based ultraviolet photodetector devices, MSM type ultraviolet photodetectors were prepared using Ga2O3 films prepared by ALD process. 10 After the device was fabricated, the IV characteristics, transient response (It) characteristics, and spectral response characteristics of the device were characterized and analyzed.
[0083] Figure 8 The IV characteristic curves of the gallium oxide-based photodetector at different annealing temperatures. Under 10V bias, the dark current of the detector at annealing temperatures of 700℃, 800℃, 900℃ and 1000℃ are 7.13×10 -10 A. 8.84×10 - 10 A. 7.36×10 -10 A and 5.94×10 -10 A, it can be seen that the dark current decreases with the increase of annealing temperature, and the size of the dark current of the photodetector mainly depends on the size of the intrinsic carrier concentration inside the Ga2O3 film. Among them, O vacancies can provide electrons as donor energy levels. Therefore, the dark current is largely affected by the concentration of O vacancies inside the film. Annealing can effectively reduce the concentration of oxygen vacancies inside the film, thereby reducing the dark current. Under 10V bias and 254nm ultraviolet light, the photocurrents of the samples annealed at 700℃, 800℃, 900℃ and 1000℃ are 1.23×10 -6 A. 1.64×10 -6 A. 1.91×10 -6 A and 1.16×10 -6 A.
[0084] In order to further analyze the effect of annealing temperature on the photoelectric conversion capability and light-to-dark current ratio (PDCR) of the GaO-based UV photodetector for incident light signals, the R and PDCR of the detector were calculated at 10V bias and different annealing temperatures. The results are shown in Figure 2. Fig. 9 As shown. When the annealing temperatures are 700℃, 800℃, 900℃ and 1000℃, the PDCR of the detector is 1719, 1853, 2595 and 1961, respectively, and the R is 12.89A / W, 17.24A / W, 20.1A / W and 12.25A / W, respectively. It can be seen that the R and PDCR of the detector increase first and then decrease with the increase of annealing temperature, and the sample annealed at 900℃ exhibits the best ultraviolet light response characteristics.
[0085] Fig.10The spectral response characteristic curve of the gallium oxide-based ultraviolet photodetector under 10V bias and annealing temperatures of 700℃, 800℃, 900℃ and 1000℃ respectively, the peak response occurs at about 254nm, which is consistent with the theoretical value of the bandgap width of Ga2O3 material (~4.9eV). It can be seen from the figure that the devices at different annealing temperatures have a large ultraviolet light responsivity, and the device annealed at 900℃ has the largest responsivity, which can be attributed to the best crystal quality of the Ga2O3 film annealed at 900℃.
[0086] Fig.11 The transient characteristic curve test results of gallium oxide-based ultraviolet photodetectors at different annealing temperatures. It can be seen that after multiple cycles of turning on / off the ultraviolet light source, the devices at different annealing temperatures all show a stable light response to the 254nm ultraviolet light source, and as the annealing temperature increases, the dark current of the detector increases first and then decreases, which is consistent with the above IV characteristic curve. Compared with the gallium oxide-based ultraviolet photodetector prepared by magnetron sputtering, the gallium oxide-based ultraviolet photodetector prepared by ALD has steeper rising and falling edges and shows a faster response speed.
[0087] In order to further analyze the effect of film annealing temperature on the spectral response speed of gallium oxide-based ultraviolet photodetectors, the normalized transient responses of gallium oxide-based ultraviolet photodetectors at different annealing temperatures were analyzed. Fig.12 It can be seen that the rise time Trise of the detector at annealing temperatures of 700℃, 800℃, 900℃ and 1000℃ is 1.04s, 1.65s, 1.9s and 2.26s respectively, and Tfall is 0.32s, 0.5s, 0.54s and 0.3s respectively. It can be seen that with the increase of annealing temperature, Trise increases slightly, and Tfall remains basically unchanged.
[0088] In order to improve the device performance of gallium oxide-based ultraviolet photodetectors from the perspective of optimizing electrode size, MSM-type ultraviolet photodetectors with different interdigital spacings were prepared using Ga2O3 films prepared by ALD process, and D was 10μm, 20μm, 40μm and 80μm respectively. After the device was prepared, the IV characteristics, transient response (It) characteristics and spectral response characteristics of the device were characterized and analyzed.
[0089] The IV characteristics of the MSM type UV detectors with different interdigital spacings prepared by ALD process based on Ga2O3 thin films were tested under 254nm, 100μW / cm2 UV light. The results are as follows Fig.13 When the external bias voltage is 10V, the photocurrents of the devices with interdigital spacings of 10μm, 20μm, 40μm, and 80μm are 1.639×10 -6A. 3.45×10 -7 A. 2.42×10 -7 A and 9.76×10 -8 A, it can be seen that with the increase of D, the device photocurrent gradually decreases, which is basically consistent with the change law of the ultraviolet photodetector prepared by Sn-doped Ga2O3 thin film deposited by magnetron co-sputtering process.
[0090] In order to further analyze the effect of interdigital spacing on the photoelectric conversion capability and signal-to-noise ratio of GaO-based UV photodetectors to external light signals, the responsivity R and light-to-dark current ratio I were used to analyze the effect of interdigital spacing on the photoelectric conversion capability and signal-to-noise ratio of GaO-based UV photodetectors to external light signals. light / I dark The calculation formula for R and I of the UV detector with different interdigital spacing under 10V external bias is light / I dark Calculate R and I light / I dark The calculation results are as follows Fig.14 As shown, the R of devices with different interdigital spacings under 10V external bias, 254nm, and 100μW / cm2 ultraviolet light are 17.24 A / W, 2.45 A / W, 1.048 A / W and 0.24A / W, the Ilight / Idark of devices with different interdigital spacings are 1665, 533, 295 and 293 respectively. It can be seen that with the decrease of interdigital spacing, R and Ilight / Idark gradually increase. Compared with the gallium oxide-based ultraviolet photodetector prepared by the thin film sample deposited by the magnetron sputtering process, the detector prepared by the Ga2O3 film deposited by the ALD process shows a stronger photoelectric conversion ability, a higher signal-to-noise ratio and a lower dark current. This is because the gallium oxide film prepared by the ALD process has a higher ultraviolet light absorption rate in the deep ultraviolet region, and the Ga2O3 film deposited by the ALD process shows better crystal quality, a denser and smoother surface morphology and fewer point defects, so that the detector prepared by the gallium oxide film prepared by the ALD process shows a stronger ultraviolet light conversion ability and a lower dark current.
[0091] Fig.15The spectral response characteristics of gallium oxide-based ultraviolet photodetectors with interdigital spacings of 10μm, 20μm, 40μm and 80μm under a bias of 10V. It can be seen that with the increase of the interdigital spacing, the responsivity of the detector gradually increases, and the peak response wavelength of the detector does not shift. Compared with the detector prepared based on the thin film deposited at a sputtering power of 30W based on the SnO2 target, the responsivity of the detector prepared based on the thin film sample prepared by the ALD method above the 310nm band and the responsivity in the visible light region are approximately 0, which is much smaller than the Sn-doped device. It can be seen that the detector prepared based on the Ga2O3 thin film prepared by the ALD method has better response wavelength selectivity and day-blind ultraviolet detector accuracy, and also shows higher light responsivity compared to the undoped device prepared based on the thin film sample prepared by the magnetron sputtering process.
[0092] The transient response characteristics of the detector prepared by ALD-deposited Ga2O3 thin film were tested under 254nm, 100μW / cm2 ultraviolet light, and 20V external bias. The results are as follows Fig.16 As shown, the switching time of the ultraviolet light source is 15s. Fig.16 It can be seen that after multiple switching of the ultraviolet light source, the photocurrent of the detectors with different interdigital spacings did not show obvious attenuation after reaching the peak value, and the photocurrent peak value of the detector did not change significantly with the increase of time.
[0093] Fig.17 The result of single-cycle normalization of the transient response characteristic curves of detectors with different interdigital spacings is shown in Figure 2. The rise time T of each device can be calculated by using the double exponential relaxation equation. rise and recovery time T fall , the results are as follows Fig.17 As shown. It can be seen that the transient response speed of the detector is significantly improved compared with the response speed of the detector prepared by the Sn-doped Ga2O3 film prepared by the magnetron sputtering process. The factors that usually limit the response speed of the photodetector include the transit time of the photogenerated carriers between the electrodes, and the capture and release of the photogenerated carriers by the internal defects of the film. Comparing the XRD and AFM test results of the Sn-doped Ga2O3 film and the Ga2O3 film deposited by the ALD process, it can be seen that the Ga2O3 film deposited by the ALD process shows a smaller FWHM, diffraction peak intensity and film surface roughness, and the Ga2O3 film prepared by the ALD process shows a more uniform and dense morphology, that is, the Ga2O3 film deposited by the ALD process shows better crystal quality and surface morphology, with a better surface state and fewer point defects, thereby reducing the hindering effect of the internal defects of the film on the photogenerated carriers in the conformity process, so that the detector shows a faster response speed.
[0094] Example 5
[0095] A method for preparing a Ga2O3 ultraviolet photodetector, the specific process is as follows:
[0096] 1. Substrate cleaning: During the experiment, a double-polished c-plane sapphire substrate was used as the substrate. Acetone, deionized water and anhydrous ethanol were used to ultrasonically clean the substrate in turn to remove impurities and oil stains on the substrate surface. Finally, the cleaned substrate was blown dry with a nitrogen gun and dried for standby use to ensure that the substrate surface was clean and dry.
[0097] 2. Thin film deposition: After the substrate is cleaned, the substrate is sent to the reaction chamber of the ALD (TFS-200, Beneq) deposition system. During the reaction process, TMGa (trimethylgallium, cold source) and O3 (99.99%) are used as Ga source and O source respectively, of which O3 is sent to the ALD reaction chamber in the form of natural volatilization under vapor pressure; high-purity nitrogen (99.9995%) is used as the carrier gas in the reaction process to clean the reaction chamber. During the reaction process, the deposition pressure of the reaction chamber is first pumped to 0.3Pa, and then the substrate temperature is heated and kept warm for 5min to ensure that the substrate temperature rises to 200℃, and then the Ga source and O source reaction precursors are sent to the reaction chamber in turn by opening the corresponding valves. In a complete reaction cycle, the time for the Ga source precursor to be injected into the reaction chamber is 0.3s, and the time for the O source precursor to be injected into the reaction chamber is 0.3s. During this period, 6s of N2 purge is required to clean the reaction chamber and remove the reaction by-products. The entire reaction needs to be repeated 1200 cycles, the preparation time is about 13 hours, and an amorphous Ga2O3 film with a thickness of about 50nm is obtained.
[0098] 3. Annealing treatment: In order to crystallize the deposited amorphous Ga2O3 film, reduce the internal defects of the film and improve the quality of the film, the prepared amorphous Ga2O3 film is subjected to high-temperature post-annealing treatment, wherein the post-annealing process parameters are: annealing temperature is 700°C, annealing atmosphere is N2, and annealing time is fixed at 2h.
[0099] 4. Detector preparation: After the Ga2O3 film is prepared, the MSM-type gallium oxide-based ultraviolet photodetector with interdigitated electrode morphology is prepared by photolithography, magnetron sputtering and lift-off processes.
[0100] Example 6
[0101] A method for preparing a Ga2O3 ultraviolet photodetector, the specific process is as follows:
[0102] 1. Substrate cleaning: During the experiment, a double-polished c-plane sapphire substrate was used as the substrate. Acetone, deionized water and anhydrous ethanol were used to ultrasonically clean the substrate in turn to remove impurities and oil stains on the substrate surface. Finally, the cleaned substrate was blown dry with a nitrogen gun and dried for standby use to ensure that the substrate surface was clean and dry.
[0103] 2. Thin film deposition: After the substrate is cleaned, the substrate is sent to the reaction chamber of the ALD (TFS-200, Beneq) deposition system. During the reaction process, TMGa (trimethylgallium, cold source) and O3 (99.99%) are used as Ga source and O source respectively, of which O3 is sent to the ALD reaction chamber in the form of natural volatilization under vapor pressure; high-purity nitrogen (99.9995%) is used as the carrier gas in the reaction process to clean the reaction chamber. During the reaction process, the deposition pressure of the reaction chamber is first pumped to 0.5Pa, and then the substrate temperature is heated and kept warm for 5min to ensure that the substrate temperature rises to 300℃, and then the Ga source and O source reaction precursors are sent to the reaction chamber in turn by opening the corresponding valves. In a complete reaction cycle, the time for the Ga source precursor to be injected into the reaction chamber is 0.7s, and the injection time for the O source precursor is 0.7s. During this period, 9s of N2 purge is required to clean the reaction chamber and remove the reaction by-products. The entire reaction needs to be repeated 2400 cycles, the preparation time is about 13 hours, and an amorphous Ga2O3 film with a thickness of about 110nm is obtained.
[0104] 3. Annealing treatment: In order to crystallize the deposited amorphous Ga2O3 film, reduce the internal defects of the film and improve the quality of the film, the prepared amorphous Ga2O3 film is subjected to high-temperature post-annealing treatment, wherein the post-annealing process parameters are: annealing temperature is 1000°C, annealing atmosphere is N2, and annealing time is fixed at 1h.
[0105] 4. Detector preparation: After the Ga2O3 film is prepared, the MSM-type gallium oxide-based ultraviolet photodetector with interdigitated electrode morphology is prepared by photolithography, magnetron sputtering and lift-off processes.
[0106] Example 7
[0107] A method for preparing a Ga2O3 ultraviolet photodetector, the specific process is as follows:
[0108] 1. Substrate cleaning: During the experiment, a double-polished c-plane sapphire substrate was used as the substrate. Acetone, deionized water and anhydrous ethanol were used to ultrasonically clean the substrate in turn to remove impurities and oil stains on the substrate surface. Finally, the cleaned substrate was blown dry with a nitrogen gun and dried for standby use to ensure that the substrate surface was clean and dry.
[0109] 2. Thin film deposition: After the substrate is cleaned, the substrate is sent to the reaction chamber of the ALD (TFS-200, Beneq) deposition system. During the reaction process, TMGa (trimethylgallium, cold source) and O3 (99.99%) are used as Ga source and O source respectively, of which O3 is sent to the ALD reaction chamber in the form of natural volatilization under vapor pressure; high-purity nitrogen (99.9995%) is used as the carrier gas in the reaction process to clean the reaction chamber. During the reaction process, the deposition pressure of the reaction chamber is first pumped to 0.4Pa, and then the substrate temperature is heated and kept warm for 5min to ensure that the substrate temperature rises to 250℃, and then the Ga source and O source reaction precursors are sent to the reaction chamber in turn by opening the corresponding valves. In a complete reaction cycle, the time for the Ga source precursor to be injected into the reaction chamber is 0.5s, and the time for the O source precursor to be injected into the reaction chamber is 0.5s. During this period, 8s of N2 purge is required to clean the reaction chamber and remove the reaction by-products. The entire reaction needs to be repeated 2000 cycles, the preparation time is about 13 hours, and an amorphous Ga2O3 film with a thickness of about 100 nm is obtained.
[0110] 3. Annealing treatment: In order to crystallize the deposited amorphous Ga2O3 film, reduce the internal defects of the film and improve the quality of the film, the prepared amorphous Ga2O3 film is subjected to high-temperature post-annealing treatment, wherein the post-annealing process parameters are: annealing temperature is 900°C, annealing atmosphere is N2, and annealing time is fixed at 1.5h.
[0111] 4. Detector preparation: After the Ga2O3 film is prepared, the MSM-type gallium oxide-based ultraviolet photodetector with interdigitated electrode morphology is prepared by photolithography, magnetron sputtering and lift-off processes.
[0112] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a Ga2O3 ultraviolet photodetector, characterized in that: The following steps are involved: S1: an amorphous Ga2O3 film is prepared on a substrate by atomic layer deposition, and the product is annealed in a nitrogen atmosphere to obtain a crystalline Ga2O3 film; S2: preparing interdigital electrodes on the crystallized Ga2O3 film by using photolithography, magnetron sputtering technology and lift-off process to obtain the Ga2O3 ultraviolet photodetector.
2. The method for preparing a Ga2O3 ultraviolet photodetector according to claim 1, characterized in that: In step S1, in the process of preparing the amorphous Ga2O3 thin film on the substrate by atomic layer deposition, trimethylgallium is used as the Ga source, O3 with a purity of 99.99% is used as the O source, and nitrogen with a purity of 99.9995% is used as the carrier gas during the deposition process.
3. The method for preparing a Ga2O3 ultraviolet photodetector according to claim 1, characterized in that: In step S1, before preparing an amorphous Ga2O3 thin film on a substrate by atomic layer deposition, the pressure of the reaction chamber is controlled to be 0.3-0.5 Pa and the temperature of the substrate is controlled to be 200-300°C.
4. The method for preparing a Ga2O3 ultraviolet photodetector according to claim 1, characterized in that: In step S1, when an amorphous Ga2O3 thin film is prepared on a substrate by atomic layer deposition, a Ga source precursor and an O source precursor are cyclically intermittently injected; the injection time of the Ga source precursor in one cycle is 0.3 to 0.7 s, and the injection time of the O source precursor is 0.3 to 0.7 s. After the injection is completed, nitrogen is used for purging before entering the next cycle.
5. The method for preparing a Ga2O3 ultraviolet photodetector according to claim 4, characterized in that: The nitrogen purge time is 6 to 9 seconds.
6. The method for preparing a Ga2O3 ultraviolet photodetector according to claim 4, characterized in that: The number of cycles is 1200-2400.
7. The method for preparing a Ga2O3 ultraviolet photodetector according to claim 1, characterized in that: The thickness of the amorphous Ga2O3 film is 50-110 nm.
8. The method for preparing a Ga2O3 ultraviolet photodetector according to claim 1, characterized in that: During the annealing process, the annealing temperature is 700-1000° C. and the annealing time is 1-2 hours.
9. A Ga2O3 ultraviolet photodetector, characterized in that: Prepared by the method according to any one of claims 1 to 8.
10. Application of the Ga2O3 ultraviolet photodetector as claimed in claim 9 in high frequency signal detection.