Novel oxidation-reduction medium for metal-air battery

By using new redox medium and electrolyte in metal air batteries, combined with the water removal treatment of 4A molecular sieve, a protective layer is formed, which solves the overpotential and dynamics of metal air batteries, and significantly improves the cycling stability and electrochemistry of the battery. performance.

CN118919958AActive Publication Date: 2024-11-08BEIJING INST OF TECH
6 Cites 0 Cited by

Patent Information

Application Number
CN202410957686.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

Smart Images

  • Figure CN118919958A_ABST
    Figure CN118919958A_ABST
Patent Text Reader

Abstract

The invention discloses a novel oxidation-reduction medium for a metal-air battery. The redox medium is added into the traditional electrolyte for the metal-air battery, so that the effect is obvious, and the overpotential of the metal-air battery can be effectively reduced. The invention also provides a specific application of the redox medium in the metal-air battery, cation groups in the redox medium can form an in-situ interface protection layer on the surface of an anode, the invasion of the oxidized redox medium and oxygen species is prevented, and the cycle stability of the battery is promoted. The novel oxidation-reduction medium provided by the invention is low in price, non-toxic and harmless, and can effectively promote the practical development of the metal-air battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of novel battery energy storage technology, and more specifically, to a novel redox medium for metal-air batteries that can effectively reduce battery overpotential. Background Art

[0002] The ultra-high theoretical energy density of metal-air batteries is believed to be able to replace traditional lithium-ion batteries and thus be integrated into electric vehicles to achieve the goal of long driving range. However, its actual energy density has been difficult to reach one-tenth of the theoretical energy density, and the current metal-air batteries are still a long way from practical application. The O2 in metal-air batteries is reduced to form metal peroxides or metal oxides through a series of coupled electron transfer steps or disproportionation reactions with metal ions. This step of the reaction involves a complex gas-liquid-solid electron transfer interface. At the cathode interface, the insulating properties and charge exchange efficiency of the reduction product are not high, resulting in a large overpotential; at the anode interface, the active oxygen species (such as O2, O2 - 、O2 2- The corrosion of the metal anode and the unstable metal interface caused by uncontrollable dendrite growth ultimately lead to serious kinetic obstacles and large battery overpotentials in metal-air batteries.

[0003] As a solution-phase catalyst, the soluble redox mediator can move freely in the electrolyte and preferentially electrochemically reduce and oxidize at the liquid-solid interface, which effectively promotes the reduction and oxidation of oxygen, thereby greatly accelerating the oxygen reaction kinetics. However, the mobility of the redox mediator will also cause the shuttle effect to react with the metal anode, which not only leads to the loss of the redox mediator and electrical energy efficiency, but also aggravates the corrosion of lithium metal. Therefore, the use of a stable redox mediator and the in-situ construction of an anode protection layer can effectively reduce the shuttle effect and give full play to the role of the redox mediator in metal-air batteries. Summary of the invention

[0004] The present invention provides a novel redox medium for metal-air batteries. The addition of the redox medium can effectively reduce the overpotential of the metal-air battery, and the in-situ formed interface protection layer can prevent the invasion of oxidized redox medium and oxygen species, thereby promoting the cycle stability of the battery.

[0005] The present invention firstly provides a method for preparing a novel redox medium electrolyte for a metal-air battery.

[0006] A second object of the present invention is to provide novel redox mediators with superior electrochemical performance in metal-air batteries.

[0007] In order to achieve the above-mentioned invention object, a series of technical solutions are adopted for implementation:

[0008] The metal-air battery is at least one of a lithium-air battery, a sodium-air battery and a potassium-air battery.

[0009] The metal-air battery electrolyte is composed of a metal salt, a solvent and a redox medium.

[0010] In the above-mentioned metal-air battery electrolyte, the metal salt is at least one of LiN(SO2CF3)2, LiC(SO2CF3)3, LiAsF6, LiCF3SO3, LiBF4, LiClO4, LiPF6, NaCF3SO3, NaC(SO2CF3)3, NaN(SO2CF3)2, NaAsF6, NaPF6, NaBF4, NaClO4, KCF3SO3, KN(SO2CF3)2, KC(SO2CF3)3, KBF4, KAsF6, and KPF6;

[0011] The solvent for dissolving the metal salt is at least one of dimethyl sulfoxide, cyclopentane, tetraethylene glycol dimethyl ether, ethylene glycol dimethyl ether, dimethylformamide, dimethylacetamide, ethyl methyl carbonate, diethyl carbonate, tetrahydrofuran, ethylene carbonate, ethyl fluoroacetate, ethyl butyrate, and propylene carbonate;

[0012] The redox mediator is C 19 H 18 PBr.

[0013] In the above-mentioned battery electrolyte, the dissolved concentration of the metal salt is 0.1-2 mol / L.

[0014] The concentration of the redox medium is 0.01-0.2 mol / L.

[0015] The present invention also provides a method for preparing the above battery electrolyte, comprising the following steps:

[0016] In an argon glove box where the H2O and O2 contents are both lower than 0.01 ppm, the metal salt is weighed and dissolved in the solvent, and then the redox medium is added and stirred for 1 day to achieve a uniform and clear state, and then the cleaned and dried 4A molecular sieve is added to fully remove water, and the prepared electrolyte is allowed to stand in the glove box for 3 to 4 days to obtain the battery electrolyte.

[0017] The application of the above battery electrolyte in the preparation of metal-air batteries also falls within the protection scope of the present invention.

[0018] The present invention further provides a metal-air battery, the electrolyte of which is the above-mentioned battery electrolyte.

[0019] The positive electrode material of the metal-air battery is at least one of Co3O4, CuO, acetylene black, nitrogen-doped graphene, single-walled carbon nanotubes, multi-walled carbon nanotubes, Super P, carbocarbon, Ketjen black, ruthenium dioxide and nickel / nickel oxide.

[0020] The negative electrode material of the metal-air battery is at least one of metallic lithium, metallic sodium, metallic potassium, LiFePO4, LiMn2O4, and LiC6.

[0021] The beneficial effects of the present invention are as follows:

[0022] The novel redox medium provided by the present invention can effectively reduce the battery reaction overpotential in the metal-air battery, and the organic cation can generate a protective layer in situ at the metal anode interface to resist the shuttle effect of the redox medium and the attack of oxygen-containing active groups, thereby inhibiting dendrite growth and corrosion; the anion can participate in promoting the reduction and oxidation reactions of oxygen and promote the reaction kinetics. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 The cyclic discharge spectrum of the lithium oxygen battery obtained in Example 1 of the present invention at a current density of 200 mA / g and a cut-off capacity of 500 mAh / g;

[0025] Figure 2 The discharge / charge curve of the lithium oxygen battery obtained in Example 1 of the present invention at a current density of 200 mA / g and a cut-off capacity of 500 mAh / g;

[0026] Figure 3 The cyclic discharge spectrum of the lithium oxygen battery obtained in Comparative Example 1 of the present invention at a current density of 200 mA / g and a cut-off capacity of 500 mAh / g;

[0027] Figure 4 The discharge / charge curve of the lithium oxygen battery obtained in Comparative Example 1 of the present invention at a current density of 200 mA / g and a cut-off capacity of 500 mAh / g; DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.

[0029] The experimental methods in the following examples are all conventional methods unless otherwise specified.

[0030] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0031] In the following embodiments:

[0032] (1) Cyclic performance test: The instrument model used is: Land, Wuhan; Test parameters: current density 200 mA / g.

[0033] (2) Preparation of metal air battery cathode:

[0034] The carbon nanotube cathode and polyvinylidene fluoride are ground in a mortar in a mass ratio of 4:1, and then an appropriate amount of N-methylpyrrolidone is dropped and fully ground to a dispersed viscous state to obtain an active slurry. The slurry is evenly coated on a porous carbon paper current collector with a coating scraper, placed in a vacuum drying oven, heated to 100°C under vacuum, and kept warm for 24 hours to obtain a dried metal-air battery cathode electrode. The electrode is cut into a circular electrode with a diameter of 11 mm using a cutting machine. The loading of a single active material is 0.20 mg, which is convenient for assembling a metal-air battery.

[0035] (3) Preparation of metal-air batteries:

[0036] Assemble the metal-air battery in an argon atmosphere with a water and oxygen content of <0.01ppm, place the shrapnel, gasket, lithium sheet, and diaphragm into the negative electrode shell in order, drop 150μL of battery electrolyte, then put the above-cut cathode electrode sheet and positive electrode shell, and press the battery with a sealing machine to obtain a button battery.

[0037] The diaphragm is a glass fiber diaphragm, model GF / D;

[0038] The button battery model size is CR 2032.

[0039] Example 1

[0040] (1) 1 M lithium bis(trifluoromethylsulfonyl)imide was weighed in an argon glove box with a water and oxygen content of <0.01 ppm, and then 10 mL of dimethyl sulfoxide solvent was added and stirred thoroughly. The mixture was stirred at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid;

[0041] (2) In an argon glove box with a water and oxygen content of <0.01 ppm, 0.1 M methyl triphenylphosphonium bromide was weighed and added to the above electrolyte, and the mixture was stirred at room temperature at a stirring speed of 200 rpm for one day to obtain a uniform colorless clear liquid;

[0042] (3) Add 4A molecular sieve to the above electrolyte, let it stand for 3-4 days until the trace water in the electrolyte is completely absorbed, and then assemble the battery for use;

[0043] The above method was used to assemble a CR2032 stainless steel button cell. The active electrode material used in this example was carbon nanotubes, the single-piece loading was 0.20 mg, and the electrolyte was the lithium-air battery electrolyte prepared in this example.

[0044] Cyclic charge and discharge performance test: Test results are as follows: Figure 1 As shown, it shows that the battery can be stably cycled for 120 cycles at room temperature.

[0045] Charge and discharge performance test: Test results are as follows Figure 2 As shown, it indicates that the overpotential of the battery is significantly reduced.

[0046] Comparative Example 1

[0047] (1) 1 M lithium bis(trifluoromethylsulfonyl)imide was weighed in an argon glove box with a water and oxygen content of <0.01 ppm, and then 10 mL of dimethyl sulfoxide solvent was added and stirred thoroughly. The mixture was stirred at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid;

[0048] (2) Add 4A molecular sieve to the above electrolyte, let it stand for 3-4 days until the trace water in the electrolyte is completely absorbed, and then assemble the battery for use;

[0049] The above method was used to assemble CR2032 stainless steel button cells. The active electrode material used in this comparative example was carbon nanotubes, the single-piece loading was 0.20 mg, and the electrolyte was the lithium-air battery electrolyte prepared in this example.

[0050] Cyclic charge and discharge performance test: Test results are as follows: Figure 3 As shown, the battery can only be stably cycled for 10 weeks at room temperature.

[0051] Charge and discharge performance test: Test results are as follows Figure 4 As shown, it shows that the overpotential of the battery is very large, indicating that the reaction kinetics are slow and the side reactions are serious.

[0052] Example 2

[0053] (1) 1 M lithium bis(trifluoromethylsulfonyl)imide was weighed in an argon glove box with a water and oxygen content of <0.01 ppm, and then 10 mL of dimethyl sulfoxide solvent was added and stirred thoroughly. The mixture was stirred at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid;

[0054] (2) In an argon glove box with a water and oxygen content of <0.01 ppm, 0.05 M methyl triphenylphosphonium bromide was weighed and added to the above electrolyte, and the mixture was stirred at room temperature at a stirring speed of 200 rpm for one day to obtain a uniform colorless clear liquid;

[0055] (3) Add 4A molecular sieve to the above electrolyte, let it stand for 3-4 days until the trace water in the electrolyte is completely absorbed, and then assemble the battery for use;

[0056] The above method was used to assemble a CR2032 stainless steel button cell. The active electrode material used in this example was carbon nanotubes, the single-piece loading was 0.20 mg, and the electrolyte was the lithium-air battery electrolyte prepared in this example.

[0057] Cyclic charge and discharge performance test: The test results show that the battery can be stably cycled for 70 weeks at room temperature.

[0058] Example 3

[0059] (1) 1 M lithium bis(trifluoromethylsulfonyl)imide was weighed in an argon glove box with a water and oxygen content of <0.01 ppm, and then 10 mL of dimethyl sulfoxide solvent was added and stirred thoroughly. The mixture was stirred at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid;

[0060] (2) In an argon glove box with a water and oxygen content of <0.01 ppm, 0.2 M methyl triphenylphosphonium bromide was weighed and added to the above electrolyte, and the mixture was stirred at room temperature at a stirring speed of 200 rpm for one day to obtain a uniform colorless clear liquid;

[0061] (3) Add 4A molecular sieve to the above electrolyte, let it stand for 3-4 days until the trace water in the electrolyte is completely absorbed, and then assemble the battery for use;

[0062] The above method was used to assemble a CR2032 stainless steel button cell. The active electrode material used in this example was carbon nanotubes, the single-piece loading was 0.20 mg, and the electrolyte was the lithium-air battery electrolyte prepared in this example.

[0063] Cyclic charge and discharge performance test: The test results show that the battery can be stably cycled for 50 weeks at room temperature.

[0064] Example 4

[0065] (1) 1 M lithium bis(trifluoromethylsulfonyl)imide was weighed in an argon glove box with a water and oxygen content of <0.01 ppm, and then 10 mL of tetraethylene glycol dimethyl ether solvent was added and stirred thoroughly. The mixture was stirred thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid;

[0066] (2) In an argon glove box with a water and oxygen content of <0.01 ppm, 0.1 M methyl triphenylphosphonium bromide was weighed and added to the above electrolyte, and the mixture was stirred at room temperature at a stirring speed of 200 rpm for one day to obtain a uniform colorless clear liquid;

[0067] (3) Add 4A molecular sieve to the above electrolyte, let it stand for 3-4 days until the trace water in the electrolyte is completely absorbed, and then assemble the battery for use;

[0068] The above method was used to assemble a CR2032 stainless steel button cell. The active electrode material used in this example was carbon nanotubes, the single-piece loading was 0.20 mg, and the electrolyte was the lithium-air battery electrolyte prepared in this example.

[0069] Cyclic charge and discharge performance test: The test results show that the battery can be stably cycled for 100 weeks at room temperature.

[0070] Example 5

[0071] (1) 1 M lithium bis(fluorosulfonyl)imide was weighed in an argon glove box with a water and oxygen content of <0.01 ppm, and then 10 mL of dimethyl sulfoxide solvent was added and stirred thoroughly. The mixture was stirred at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid;

[0072] (2) In an argon glove box with a water and oxygen content of <0.01 ppm, 0.1 M methyl triphenylphosphonium bromide was weighed and added to the above electrolyte, and the mixture was stirred at room temperature at a stirring speed of 200 rpm for one day to obtain a uniform colorless clear liquid;

[0073] (3) Add 4A molecular sieve to the above electrolyte, let it stand for 3-4 days until the trace water in the electrolyte is completely absorbed, and then assemble the battery for use;

[0074] The above method was used to assemble a CR2032 stainless steel button cell. The active electrode material used in this example was carbon nanotubes, the single-piece loading was 0.20 mg, and the electrolyte was the lithium-air battery electrolyte prepared in this example.

[0075] Cyclic charge and discharge performance test: The test results show that the battery can be stably cycled for 110 weeks at room temperature.

[0076] The above-described embodiments of the present invention do not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A novel redox medium for metal-air batteries, characterized in that: The following steps are included.

2. Introduce the application of redox mediators in the preparation of metal-air battery electrolytes, including solvents, metal salts, and redox mediators.

3. The metal-air battery electrolyte according to claim 2, characterized in that: The electrolyte includes a solvent, a metal salt, and a redox mediator.

4. The metal-air battery electrolyte according to claims 2 and 3, characterized in that: The metal salt is at least one of LiN(SO2CF3)2, LiC(SO2CF3)3, LiAsF6, LiCF3SO3, LiBF4, LiClO4, LiPF6, NaCF3SO3, NaC(SO2CF3)3, NaN(SO2CF3)2, NaAsF6, NaPF6, NaBF4, NaClO4, KCF3SO3, KN(SO2CF3)2, KC(SO2CF3)3, KBF4, KAsF6, and KPF6; The solvent for dissolving the metal salt is at least one of dimethyl sulfoxide, cyclopentane, tetraethylene glycol dimethyl ether, ethylene glycol dimethyl ether, dimethylformamide, dimethylacetamide, ethyl methyl carbonate, diethyl carbonate, tetrahydrofuran, ethylene carbonate, ethyl fluoroacetate, ethyl butyrate, and propylene carbonate; The redox mediator is C 19 H 18 PBr.

5. The novel redox medium for metal-air battery according to claims 2-4, characterized in that: The dissolved concentration of the metal salt is 0.1 to 2 mol / L. The concentration of the redox medium is 0.01-0.2 mol / L.

6. The method for preparing a novel redox medium for a metal-air battery according to any one of claims 2 to 5, comprising the following steps: In an argon glove box where the H2O and O2 contents are both lower than 0.01 ppm, the metal salt is weighed and dissolved in the solvent, and then the redox medium is added and stirred for 1 day to achieve a uniform and clear state, and then the cleaned and dried 4A molecular sieve is added to fully remove water, and the prepared electrolyte is allowed to stand in the glove box for 3 to 4 days to obtain the battery electrolyte.

7. Use of the battery electrolyte according to any one of claims 2 to 5 in the preparation of a metal-air battery.

8. A metal-air battery, wherein the electrolyte used is the metal-air battery electrolyte as claimed in any one of claims 2 to 6.

9. The use according to claim 7 or the metal-air battery according to claim 8, characterized in that: The positive electrode material of the metal-air battery is at least one of Co3O4, CuO, acetylene black, nitrogen-doped graphene, single-walled carbon nanotubes, multi-walled carbon nanotubes, Super P, carbocarbon, Ketjen black, ruthenium dioxide and nickel / nickel oxide; The negative electrode material of the metal-air battery is at least one of metallic lithium, metallic sodium, metallic potassium, LiFePO4, LiMn2O4, and LiC6.

Citation Information

Patent Citations

  • Redox-type fuel cell

    CN106463756A

  • Functional electrolyte additive for lithium metal air battery

    CN115692851A

  • Low-temperature metal-air battery electrolyte with corrosion inhibitor introduced

    CN117317470A

  • Metal-air battery

    JP2020149923A

  • Metal air battery

    JP2021111574A