Etching method regulated porous cement-based diaphragm as well as preparation method and application thereof
The pore structure of the cement-based separator is regulated by etching method, and the acidic solution is used to dissolve the components of the cement-based separator, which solves the problem of insufficient porosity and pore connectivity of the cement-based separator, and significantly improves its ionic conductivity and electrochemical energy storage performance. .
Patent Information
- Application Number
- CN202410994135.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing cement-based electrochemical energy storage membrane has small porosity, poor pore connectivity and low ionic conductivity, resulting in poor performance in energy storage applications.
The pore structure of the cement-based separator is controlled by etching method, and the components of the cement slurry are dissolved through an acid solution, the pore size and pore ratio are expanded, and the pore connectivity is improved, thereby improving ionic conductivity.
It significantly improves the ionic conductivity and electrochemical energy storage performance of cement-based separators, solves the problems of insufficient porosity and pore connectivity, and provides more efficient energy storage characteristics.
Smart Images

Figure CN118920021A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery diaphragms, and in particular to a method for preparing a porous cement-based diaphragm regulated by an etching method and an application of the diaphragm in electrochemical energy storage. Background Art
[0002] With the rapid population growth and deepening industrialization, global fossil energy is facing serious problems such as energy depletion and environmental pollution. Against this background, renewable energy represented by solar energy and wind energy has ushered in new development opportunities. However, renewable energy is characterized by large volatility, strong randomness, and intermittency, and it is difficult for its peak power generation to coincide with the peak power consumption. The energy storage system can smooth the volatility of renewable energy power generation, reduce energy waste, and promote the consumption of new energy. Therefore, the development and application of energy storage technology has become the key to promoting the development of renewable energy. The current energy storage technologies include mechanical energy storage, electrochemical energy storage, electromagnetic energy storage, and electrochemical energy storage. Among them, electrochemical energy storage is increasingly widely used in the field of energy storage due to its advantages such as reliability, economy, long life cycle, large capacity, less restricted by terrain, flexible operation, and fast response.
[0003] The electrochemical energy storage system consists of electrodes and diaphragms, which are assembled into a sandwich configuration according to the "electrode-diaphragm-electrode" structure. The diaphragm isolates the positive and negative electrodes to prevent short circuits and only allows ions to pass through to form a charge and discharge circuit. It must have the basic properties of electrical insulation, high mechanical strength, rich pore structure, and high ionic conductivity. However, the mechanical strength of existing commercial electrochemical energy storage diaphragms is not high and is easily penetrated by dendrites, which leads to safety problems. Therefore, the development of new diaphragm materials is an important means to promote the further development of energy storage technology and new energy.
[0004] The non-flammability, electrical insulation, high mechanical properties and pore-rich properties of cement-based materials make them potential as diaphragms. The ion transport performance of cement-based diaphragms is a key factor affecting their electrochemical energy storage. The existing methods for improving the ion transport performance of cement-based diaphragms include adding polymers (such as polyacrylic acid PAA, polyvinyl alcohol PVA, etc.) and pore structure regulation. Polymers can provide additional channels for ion transport, but polymers are prone to agglomeration during the incorporation process and are prone to dehydration due to the loss of pore solution, resulting in uneven pores inside the diaphragm and decreased ion transport performance. Pore structure regulation is a method to increase the porosity of cement-based diaphragms, increase pore connectivity, improve pore size distribution, and thus improve their ion transport performance. This method is simple and convenient to operate, and the methods include changing the mix ratio, changing the curing conditions, and entraining air. Changing the mix ratio and curing conditions can only increase the porosity of the material to a limited extent, and its ion transport performance is still poor. Although air entrainment can improve the porosity and ion transmission performance of the material by introducing a large number of bubbles, the location and size of the bubbles are random, so this method has poor controllability of the pore structure of the material. The present invention provides a new pore structure control method, which applies the etching method to cement-based diaphragms, and uses an acidic solution to dissolve the components of the cement-based diaphragm itself to leave holes, thereby achieving the purpose of expanding the pore size, increasing the porosity and improving the pore connectivity, thereby effectively improving its ion transmission performance and electrochemical energy storage performance. This method can more effectively control the pore structure characteristics of cement-based diaphragms by optimizing parameters such as the water-cement ratio and mass loss of cement slurry. Summary of the invention
[0005] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a porous cement-based membrane regulated by etching, which method can improve the porosity and pore connectivity of cement slurry, thereby improving its ionic conductivity; another purpose of the present invention is to provide a cement-based membrane; another purpose of the present invention is to provide an electrochemical energy storage device.
[0006] Technical solution: In order to solve the problems of small porosity, poor pore connectivity and low ion conductivity of existing cement-based materials, the present invention provides a preparation method of porous cement-based battery separator based on etching method, and applies it in electrochemical energy storage devices.
[0007] The invention discloses a cement-based diaphragm, on which a plurality of etched pores are distributed. The etched pores are obtained by etching a cement paste sheet with an acid solution, and the mass loss of the cement paste sheet is 5-40%. The cement paste sheet is further enlarged in porosity, pore size and pore connectivity by etching.
[0008] Furthermore, the acidic solution is any one or a mixture of 1-5 mol / L ammonium chloride solution, 1-6 mol / L ammonium nitrate solution or 0.1-1 mol / L hydrochloric acid solution.
[0009] Furthermore, the components of the etched cement paste slice include one or more of calcium silicate hydrate, calcium hydroxide, calcium carbonate, calcium sulfonate, etc.
[0010] On the other hand, the present invention provides a method for preparing the above-mentioned cement-based diaphragm, firstly, soaking a cement slurry sheet in water and placing it in a negative pressure environment to be fully saturated with water, then soaking the saturated cement slurry sheet in an acidic solution to etch away the components of the cement slurry, monitoring the mass loss of the cement slurry sheet, soaking the etched cement slurry sheet in water to remove the etching solution, and then drying to obtain the cement-based diaphragm.
[0011] Furthermore, the immersion time in water is 1 to 3 days, and the negative pressure is -0.05 to -0.1 MPa;
[0012] Furthermore, the water-cement ratio of the cement paste is 0.3-0.7, preferably 0.5; the stirring time is 60-90s, the temperature of the curing room is 18-22°C, the relative humidity is above 95%, and the age is 1-180d, preferably 28-56d.
[0013] Furthermore, the soaking time in water is 1 to 7 days; the drying is one or more of natural drying, vacuum drying, freeze drying or microwave drying, and the drying time is 1 to 14 days.
[0014] Specifically, the preparation method of the cement-based diaphragm comprises the following steps:
[0015] (1) Preparation of cement slurry slices: Cement and water are mixed and stirred and poured into a mold, and then polished after curing to obtain cement slurry slices;
[0016] (2) Acid solution etching: First, the cement paste sheet is immersed in water and placed in a negative pressure environment to be fully saturated with water, and then the saturated cement paste sheet is immersed in an acid solution to etch away the components of the cement paste, and the mass loss of the cement paste sheet is monitored to obtain a cement-based membrane with a desired porosity;
[0017] (3) Drying: The etched cement paste slice is soaked in water to remove the etching solution, and then dried to obtain a cement-based diaphragm.
[0018] Furthermore, in step (1), the polishing method is to use one or more of sandpaper, automatic polishing machine and manual polishing machine.
[0019] Furthermore, in step (1), the thickness of the cement slurry sheet is 0.4-5.0 mm.
[0020] On the other hand, the present invention provides an electrochemical energy storage device, which includes the above-mentioned cement-based diaphragm, two pole ears, a positive electrode and a negative electrode, wherein the pole ears are fixedly connected to the positive and negative electrodes, respectively, and the cement-based diaphragm is immersed in the electrolyte under negative pressure and is placed between the positive and negative electrodes to form a sandwich structure.
[0021] Furthermore, the cement-based diaphragm forms a sandwich structure with the positive and negative electrodes and is then sealed, wherein the sealing method is one of vacuum packaging, epoxy coating or paraffin coating.
[0022] Furthermore, the material of the tab is one or more of aluminum, stainless steel, nickel, titanium, etc.
[0023] Furthermore, the electrolyte immersion time is 1 to 28 days.
[0024] Furthermore, the electrolyte is one or more of soluble salt solutions such as zinc sulfate, zinc acetate, zinc nitrate, manganese sulfate, potassium hydroxide, and sodium hydroxide.
[0025] Furthermore, the positive and negative electrodes are electrodes made of metal foil (zinc, copper, platinum, etc.) or active materials.
[0026] Furthermore, the specific method for preparing the active material electrode is: firstly, the active material, the conductive agent and the binder are put into a mortar and ground evenly, then N-methylpyrrolidone is added and stirred rapidly, and finally, the obtained slurry is evenly coated on a conductive carrier, and the active material electrode is obtained after drying.
[0027] Specifically, the specific method for preparing the active material electrode is: first, the active material, the conductive agent and the binder are put into a mortar according to the mass ratio and fully ground evenly, then N-methylpyrrolidone is added according to the liquid-solid mass ratio and quickly stirred, and finally the obtained slurry is evenly coated on a conductive carrier and placed in a blast drying oven for drying.
[0028] Furthermore, the active material is one or more of activated carbon, graphene, redox graphene, manganese dioxide or nano carbon black.
[0029] Furthermore, the conductive agent is one or more of acetylene black, Ketjen black, conductive graphite or nano-carbon fiber.
[0030] Furthermore, the binder is one or more of polyvinylidene fluoride, sodium alginate, polyvinyl alcohol, hydroxymethyl cellulose and the like.
[0031] Furthermore, the mass ratio ranges from (75-85):(5-15):(5-15), and the preferred mass ratio is 8:1:1.
[0032] Furthermore, the liquid-to-solid mass ratio is 2-7.
[0033] Furthermore, the slurry is evenly applied by a scraper, a shovel, a four-blade wet film preparation device or an automatic coating machine.
[0034] Furthermore, the carrier is one or more of metal materials such as stainless steel, copper, titanium, nickel, etc. in foil, mesh or foam form.
[0035] Furthermore, the loading amount of the active substance is 0.5 to 30 mg / cm 2 .
[0036] Furthermore, the drying temperature is 55-65° C., and the drying time is 4-36 hours.
[0037] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) Cement paste is a composite material composed of multiple phases, and its constituent phases are easily dissolved by acid. When the pore structure of cement paste is regulated by etching, the constituent phases of the cement paste itself can be used as porogens, without adding additional porogens. Subsequently, the porogens are dissolved by acid solution to leave holes, and the process is simplified;
[0038] (2) Compared with hydrostatic etching, acid solution etching can quickly dissolve some components of cement paste, thus saving time;
[0039] (3) The present invention regulates the pore structure of cement-based diaphragms from a microscopic perspective. Acid solution etching can improve the porosity and pore connectivity of cement paste, expand the ion transmission channel, and further improve the ionic conductivity of cement paste, thereby effectively improving the energy storage characteristics of the material and providing a new idea for alleviating the energy crisis.
[0040] (4) By optimizing the water-cement ratio, age, thickness and mass loss of cement paste, the pore structure parameters of cement-based diaphragms can be effectively regulated, and the application prospects are broad;
[0041] (5) The method of the present invention is simple and reasonable, easy to operate, has low raw material cost, is environmentally friendly, and has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 A schematic diagram of the structure of the energy storage device provided by the present invention, wherein: 1. a pole ear; 2. a positive electrode; 3. a negative electrode; 4. a cement-based diaphragm; 5. an energy storage device;
[0043] Figure 2 The AC impedance spectrum, charge-discharge curve and long cycle of Example 1 obtained by the present invention;
[0044] Figure 3The AC impedance spectrum, charge-discharge curve and long cycle of Example 2 obtained by the present invention;
[0045] Figure 4 The AC impedance spectrum, charge-discharge curve and long cycle of Example 3 obtained by the present invention;
[0046] Figure 5 The AC impedance spectrum, charge-discharge curve and long cycle of Example 4 obtained by the present invention;
[0047] Figure 6 The AC impedance spectrum, charge-discharge curve and long cycle of Example 5 obtained by the present invention;
[0048] Figure 7 The AC impedance spectrum, charge-discharge curve and long cycle of Example 6 obtained by the present invention;
[0049] Figure 8 The AC impedance spectrum, charge-discharge curve and long cycle of Example 7 obtained by the present invention;
[0050] Fig. 9 The AC impedance spectrum, charge-discharge curve and long cycle of Example 8 obtained by the present invention;
[0051] Fig.10 The AC impedance spectrum, charge-discharge curve and long cycle of Example 9 obtained by the present invention;
[0052] Fig.11 The AC impedance spectrum, charge-discharge curve and long cycle of Example 10 obtained by the present invention;
[0053] Fig.12 The AC impedance spectrum, charge-discharge curve and long cycle of Example 11 obtained by the present invention;
[0054] Fig.13 The AC impedance spectrum, charge-discharge curve and long cycle of Example 12 obtained by the present invention;
[0055] Fig.14 The AC impedance spectrum, charge-discharge curve and long cycle of Example 13 obtained by the present invention;
[0056] Fig.15 The AC impedance spectrum, charge-discharge curve and long cycle of Example 14 obtained by the present invention;
[0057] Fig.16 The AC impedance spectrum, charge-discharge curve and long cycle of Example 15 obtained by the present invention;
[0058] Fig.17The AC impedance spectrum, charge-discharge curve and long cycle of Example 16 obtained by the present invention;
[0059] Fig.18 The AC impedance spectrum, charge-discharge curve and long cycle of Example 17 obtained by using the present invention. DETAILED DESCRIPTION
[0060] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0061] like Figure 1 As shown, an embodiment of the present invention provides an electrochemical energy storage device 5 including a pole ear 1, a positive electrode 2, a negative electrode 3, and a cement-based diaphragm 4 disposed between the two electrodes after etching and soaked with an electrolyte; wherein the pole ear 1 is fixedly connected to the positive electrode 2 and the negative electrode 3, respectively, the cement-based diaphragm 4 is immersed in the electrolyte under negative pressure, and is placed between the positive electrode 2 and the negative electrode 3 to form a sandwich structure, and the positive and negative electrodes are electrodes made of metal foil or active substances.
[0062] Example 1
[0063] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, curing was carried out in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95% for 5 days. The specimen was polished into a 1.0 mm thin slice, and soaked in deionized water for 1 day, then placed in a 0.1 mol / L hydrochloric acid solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 5%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 40.4%.
[0064] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0065] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0066] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and soak cement-based diaphragm in zinc sulfate solution to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Figure 2 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.29S / m. The maximum specific capacity was 66.9mWh / g, and the energy decay was 13.1% after 220 cycles.
[0067] Example 2
[0068] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 7 days, the acid etching solution is 1.25 mol / L ammonium nitrate solution, and the mass loss of the specimen is 20%.
[0069] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 7 days in a curing room at a temperature of 20±2°C and a relative humidity of more than 95%. The specimen was polished into a 1.0 mm thin slice, and soaked in deionized water for 1 day, then placed in a 1.25 mol / L ammonium nitrate solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 20%. Finally, it was dried in a vacuum drying oven at 45°C for 7 days to obtain a cement-based diaphragm with a porosity of 67.4%.
[0070] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0071] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0072] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and soak cement-based diaphragm in zinc sulfate solution to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Figure 3 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.47S / m. The maximum specific capacity was 102mWh / g, and the energy decay was 13.4% after 340 cycles.
[0073] Example 3
[0074] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 7 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 20%.
[0075] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 7 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 20%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 64.1%.
[0076] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0077] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0078] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and soak cement-based diaphragm in zinc sulfate solution to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Figure 4 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.51S / m. The maximum specific capacity was 69.9mWh / g, and the energy decay was 10.4% after 1050 cycles.
[0079] Example 4
[0080] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 7 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 28%.
[0081] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 7 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1.0 mm thin slice, soaked in deionized water for 1 day, and then placed in a 4 mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 28%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 68.5%.
[0082] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0083] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0084] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and soak cement-based diaphragm in zinc sulfate solution to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Figure 5 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 1.39S / m. The maximum specific capacity was 89.9mWh / g, and the energy decay was 20.4% after 925 cycles.
[0085] Example 5
[0086] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 7 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 14%.
[0087] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 7 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1.0 mm thin slice, soaked in deionized water for 1 day, and then placed in a 4 mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 14%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 55.9%.
[0088] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0089] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0090] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and soak cement-based diaphragm in zinc sulfate solution to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Figure 6 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.364S / m. The maximum specific capacity was 69mWh / g, and the energy decay was 7.2% after 850 cycles.
[0091] Example 6
[0092] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 7 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 18%.
[0093] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 7 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1.0 mm thin slice, soaked in deionized water for 1 day, and then placed in a 4 mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 18%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 61%.
[0094] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0095] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0096] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and soak cement-based diaphragm in zinc sulfate solution to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Figure 7 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.492S / m. The maximum specific capacity was 79.6mWh / g, and the energy decay was 4.1% after 800 cycles.
[0097] Example 7
[0098] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 7 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 24%.
[0099] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 7 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1.0 mm thin slice, soaked in deionized water for 1 day, and then placed in a 4 mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 24%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 62.3%.
[0100] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0101] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0102] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and soak cement-based diaphragm in zinc sulfate solution to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Figure 8 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.834S / m. The maximum specific capacity was 86.7mWh / g, and the energy decay was 7% after 948 cycles.
[0103] Example 8
[0104] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 14 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 24%.
[0105] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 14 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1.0 mm thin slice, and soaked in deionized water for 1 day, then placed in a 4 mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 24%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 69%.
[0106] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0107] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0108] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and cement-based diaphragm soaked in zinc sulfate to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig. 9 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.98S / m. The maximum specific capacity was 83.8Wh / g, and the energy decay was 6% after 984 cycles.
[0109] Example 9
[0110] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 14 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 28%.
[0111] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 14 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1.0 mm thin slice, and soaked in deionized water for 1 day, then placed in a 4 mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 28%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 70%.
[0112] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0113] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0114] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and cement-based diaphragm soaked in zinc sulfate to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.10 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 1.465S / m. The maximum specific capacity was 84.1mWh / g, and the energy decay was 9.2% after 989 cycles.
[0115] Example 10
[0116] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that in this embodiment, the specimen is cured for 28 days, the specimen is polished into a 0.8 mm thin slice, and the acid etching solution is a 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 16%. The energy storage device of this embodiment is configured the same as that of embodiment 1.
[0117] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 0.8mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 16%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 56.3%.
[0118] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0119] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0120] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and cement-based diaphragm soaked in zinc sulfate to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.11 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 0.39S / m. The maximum specific capacity was 85.8mWh / g, and the energy decay was 15% after 270 cycles.
[0121] Embodiment 11
[0122] The difference between the cement-based membrane manufacturing of this embodiment and embodiment 1 is that: in this embodiment, the specimen is cured for 28 days, the specimen is polished into a 0.8 mm thin slice, and the acid etching solution is a 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 30%. The energy storage device of this embodiment is configured the same as that of embodiment 1.
[0123] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 0.8mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 30%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 70.1%.
[0124] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0125] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0126] Energy storage device: Use activated carbon electrode as positive electrode, zinc electrode as negative electrode, and cement-based diaphragm soaked in zinc sulfate to form a hybrid supercapacitor. Immerse the dry cement-based diaphragm in 2mol / L zinc sulfate solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the positive and negative electrodes, then place the cement-based diaphragm soaked in electrolyte between the two electrodes, fix it with tape to form a sandwich structure, and seal it. Finally, test the frequency range of 0.1~10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.12 ; In the voltage window of 0.2~1.8V, the current density is 0.4mA / cm 2 The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of , and the calculated ion conductivity of the cement-based diaphragm was 1.42S / m. The maximum specific capacity was 92mWh / g, and the energy decay was 5% after 110 cycles.
[0127] Example 12
[0128] The difference between the cement-based diaphragm preparation of this embodiment and that of embodiment 1 is that in this embodiment, the curing is performed for 28 days, and the acid etching solution is a 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 20%.
[0129] The configuration of the energy storage device of this embodiment differs from that of Embodiment 1 in that activated carbon electrodes are used as positive and negative electrodes, and a cement-based diaphragm is soaked in potassium hydroxide solution to form a supercapacitor.
[0130] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 20%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 58.2%.
[0131] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0132] Energy storage device: Use activated carbon electrodes as positive and negative electrodes, and soak cement-based diaphragms in potassium hydroxide solution to form supercapacitors. Immerse the dry cement-based diaphragm in 2 mol / L potassium hydroxide solution and place it in a negative pressure environment of -0.1Mpa for 14 days. First, fix the tabs to the electrodes, then place the cement-based diaphragm soaked in electrolyte between the positive and negative electrodes, and fix it with tape to form a sandwich structure for sealing. Finally, test the frequency range of 0.1 to 10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.13 ; In the voltage window of 0~1.0V, the current density is 0.4mA / cm 2 The constant current charge and discharge performance and cycle performance of the supercapacitor were tested under the conditions of Fig.13 and Fig.13 .according to Fig.13 The calculated ionic conductivity of the cement-based membrane is 3.69S / m. Fig.13 The maximum specific capacity is 17.3mWh / g, and the energy decay is 46% after 880 cycles.
[0133] Example 13
[0134] The difference between the cement-based diaphragm preparation of this embodiment and that of embodiment 1 is that in this embodiment, the curing is performed for 28 days, and the acid etching solution is a 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 24%.
[0135] The difference between the configuration of the energy storage device of this embodiment and that of Embodiment 1 is that a manganese dioxide electrode is used as the positive electrode, a graphene electrode is used as the negative electrode, and a cement-based diaphragm is soaked in potassium hydroxide solution to form a supercapacitor.
[0136] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 24%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 60.5%.
[0137] Manganese dioxide electrode preparation: 350 mg manganese dioxide, 100 mg acetylene black and 50 mg polyvinylidene fluoride were put into a mortar and ground for 10 min. 1700 μL N-methylpyrrolidone was added to the mortar and stirred rapidly to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm) and then placed in a 60°C air drying oven for 24 h. The slurry was cut into manganese dioxide electrodes with a diameter of 12 mm using a tablet press. The activated carbon loading was about 1.05 mg / cm 2 .
[0138] Preparation of graphene electrode: 400 mg of graphene, 50 mg of acetylene black and 50 mg of polyvinylidene fluoride were put into a mortar and ground for 10 min. 2000 μL of N-methylpyrrolidone was added to the mortar and stirred rapidly to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm) and then placed in a 60°C forced air drying oven for 24 h. The graphene electrode was cut into 12 mm in diameter with a tablet press. The activated carbon loading was about 1.63 mg / cm 2 .
[0139] Energy storage device: A supercapacitor is formed by using a manganese dioxide electrode as the positive electrode, a graphene electrode as the negative electrode, and a cement-based diaphragm soaked in potassium hydroxide solution. The dried cement-based diaphragm is immersed in a 6 mol / L potassium hydroxide solution and placed in a negative pressure environment of -0.1 MPa for 14 days. First, the tabs are fixedly connected to the electrodes, and then the cement-based diaphragm soaked in electrolyte is placed between the positive and negative electrodes, and the tape is fixed to form a sandwich structure for sealing. Finally, the test frequency range is 0.1 to 10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.14 ; In the voltage window of 0~1.0V, the current density is 0.4mA / cm 2 The constant current charge and discharge performance and cycle performance of the supercapacitor were tested under the conditions of Fig.14 and Fig.14 .according to Fig.14 , the calculated ionic conductivity of the cement-based membrane is 5.89S / m. Fig.14 The maximum specific capacity is 13.6mWh / g, and the energy decay is 25% after 1140 cycles.
[0140] Embodiment 14
[0141] The preparation steps of the cement-based diaphragm in this embodiment are the same as those in Example 13, and the porosity of the obtained cement-based diaphragm is slightly different, which is caused by different experimental batches.
[0142] The difference between the configuration of the energy storage device of this embodiment and that of Embodiment 13 is that a graphene electrode is used as the positive electrode, an activated carbon electrode is used as the negative electrode, and a cement-based diaphragm is soaked in potassium hydroxide solution to form a supercapacitor.
[0143] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 24%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 61.1%.
[0144] Preparation of graphene electrode: 400 mg of graphene, 50 mg of acetylene black and 50 mg of polyvinylidene fluoride were put into a mortar and ground for 10 min. 2000 μL of N-methylpyrrolidone was added to the mortar and stirred rapidly to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm) and then placed in a 60°C forced air drying oven for 24 h. The graphene electrode was cut into 12 mm in diameter with a tablet press. The activated carbon loading was about 1.63 mg / cm 2 .
[0145] Preparation of activated carbon electrode: 400 mg activated carbon, 50 mg acetylene black and 50 mg polyvinylidene fluoride were ground in a mortar for 10 min, 1800 μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm), and then placed in a 60°C air drying oven for 24 hours. It was cut into activated carbon electrodes with a diameter of 12 mm using a tablet press, and the activated carbon loading was about 2.45 mg / cm 2 .
[0146] Energy storage device: A supercapacitor is formed by using a graphene electrode as the positive electrode, an activated carbon electrode as the negative electrode, and a cement-based diaphragm soaked in potassium hydroxide solution. The dried cement-based diaphragm is immersed in a 6 mol / L potassium hydroxide solution and placed in a negative pressure environment of -0.1 MPa for 14 days. First, the tabs are fixedly connected to the electrodes, and then the cement-based diaphragm soaked in electrolyte is placed between the positive and negative electrodes, and the tape is used to fix the sandwich structure for sealing. Finally, the test frequency range is 0.1 to 10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.15 ; In the voltage window of 0~1.0V, the current density is 0.4mA / cm 2 The constant current charge and discharge performance and cycle performance of the supercapacitor were tested under the conditions of Fig.15 and Fig.15 .according to Fig.15 , the calculated ionic conductivity of the cement-based membrane is 2.58S / m. Fig.15 The maximum specific capacity is 20.7mWh / g, and the energy decay is 15% after 1400 cycles.
[0147] Embodiment 15
[0148] The preparation steps of the cement-based diaphragm in this embodiment are the same as those in Example 13, and the porosity of the obtained cement-based diaphragm is slightly different, which is caused by different experimental batches.
[0149] The difference between the configuration of the energy storage device of this embodiment and that of Embodiment 13 is that graphene electrodes are used as positive and negative electrodes, and a cement-based diaphragm is soaked in potassium hydroxide solution to form a supercapacitor.
[0150] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 24%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 60.85%.
[0151] Preparation of graphene electrode: 400 mg of graphene, 50 mg of acetylene black and 50 mg of polyvinylidene fluoride were put into a mortar and ground for 10 min. 2000 μL of N-methylpyrrolidone was added to the mortar and stirred rapidly to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm) and then placed in a 60°C forced air drying oven for 24 h. The graphene electrode was cut into 12 mm in diameter with a tablet press. The activated carbon loading was about 1.63 mg / cm 2 .
[0152] Energy storage device: With graphene electrodes as positive and negative electrodes, cement-based diaphragms are soaked in potassium hydroxide solution to form supercapacitors. The dried cement-based diaphragms are immersed in 6 mol / L potassium hydroxide solution and placed in a negative pressure environment of -0.1 Mpa for 14 days. First, the tabs are fixedly connected to the electrodes, and then the cement-based diaphragms soaked in electrolyte are placed between the positive and negative electrodes, and fixed with tape to form a sandwich structure for sealing. Finally, the test frequency range is 0.1 to 10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.16 ; In the voltage window of 0~1.0V, the current density is 0.4mA / cm 2 The constant current charge and discharge performance and cycle performance of the supercapacitor were tested under the conditions of Fig.16 and Fig.16 .according to Fig.16The calculated ionic conductivity of the cement-based membrane is 3.48S / m. Fig.16 The maximum specific capacity is 13.1mWh / g, and the energy decay is 10% after 300 cycles.
[0153] Example 16
[0154] The difference between the cement-based membrane manufacturing of this embodiment and that of embodiment 1 is that the curing time of this embodiment is 28 days, the acid etching solution is 4 mol / L ammonium chloride solution, and the mass loss of the specimen is 28%.
[0155] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 28%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 68.1%.
[0156] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0157] Preparation of graphene electrode: 400 mg of graphene, 50 mg of acetylene black and 50 mg of polyvinylidene fluoride were put into a mortar and ground for 10 min. 2000 μL of N-methylpyrrolidone was added to the mortar and stirred rapidly to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10 μm) and then placed in a 60°C forced air drying oven for 24 h. The graphene electrode was cut into 12 mm in diameter with a tablet press. The activated carbon loading was about 1.63 mg / cm 2 .
[0158] Energy storage device: A supercapacitor is formed by using a graphene electrode as the positive electrode, a zinc foil as the negative electrode, and a cement-based diaphragm soaked in zinc sulfate solution. The dry cement-based diaphragm is immersed in a 2 mol / L zinc sulfate solution and placed in a negative pressure environment of -0.1 MPa for 14 days. First, the tabs are fixedly connected to the electrodes, and then the cement-based diaphragm soaked in electrolyte is placed between the positive and negative electrodes, and the tape is fixed to form a sandwich structure for sealing. Finally, the test frequency range is 0.1 to 10 6 The AC impedance spectrum is tested under the condition of Hz, see Fig.17 ; In the voltage window of 0.2~1.8V, the current density is 0.32mA / cm 2The constant current charge-discharge performance and cycle performance of the hybrid capacitor were tested under the conditions of . The calculated ionic conductivity of the cement-based diaphragm is 0.63S / m. The maximum specific capacity is 50.5mWh / g, and the energy decay is 16% after 880 cycles.
[0159] Embodiment 17
[0160] The preparation steps of the cement-based diaphragm in this embodiment are the same as those in Example 16, and the porosity of the obtained cement-based diaphragm is slightly different, which is caused by different experimental batches.
[0161] The configuration of the energy storage device of this embodiment differs from that of Embodiment 16 in that a manganese dioxide electrode is used as the positive electrode, a zinc foil is used as the negative electrode, and a cement-based diaphragm is soaked in a mixed solution of zinc sulfate solution and manganese sulfate to form a battery.
[0162] Preparation of cement-based diaphragm: Deionized water and silicate cement were stirred in a mixing pot at a water-cement ratio of 0.5 for 60 seconds, then poured into a mold with an inner diameter of 13 mm and a depth of 5 mm. After hardening for 1 day, demoulding, the mold was removed and cured for 28 days in a curing room with a temperature of 20±2℃ and a relative humidity of more than 95%. The specimen was polished into a 1mm thin slice, soaked in deionized water for 1 day, and then placed in a 4mol / L ammonium chloride solution. The mass was weighed every 30 minutes and the mass loss was calculated until the mass loss of the specimen reached 28%. Finally, it was dried in a vacuum drying oven at 45℃ for 7 days to obtain a cement-based diaphragm with a porosity of 69%.
[0163] Zinc electrode preparation: Use a sheet press to cut the zinc foil into zinc electrodes with a diameter of 12 mm.
[0164] Preparation of manganese dioxide positive electrode: 350mg manganese dioxide, 100mg acetylene black and 50mg polyvinylidene fluoride were put into a mortar and ground for 10min, 1700μL N-methylpyrrolidone was added to the mortar, and the slurry was quickly stirred to obtain a slurry. The slurry was evenly coated on a 200-mesh stainless steel mesh with a film applicator (10μm), and then placed in a 60℃ forced air drying oven for 24h, and cut into a manganese dioxide positive electrode with a diameter of 12mm using a tablet press. The activated carbon loading was about 1.05mg / cm 2 .
[0165] Energy storage device: With manganese dioxide electrode as positive electrode, zinc foil as negative electrode, and cement-based diaphragm soaked in a mixed solution of zinc sulfate solution and manganese sulfate, a battery is formed. The dry cement-based diaphragm is immersed in a mixed solution of 2 mol / L zinc sulfate and 0.1 mol / L manganese sulfate, and placed in a negative pressure environment of -0.1Mpa for 14 days. First, the tabs are fixedly connected to the electrodes, and then the cement-based diaphragm soaked with electrolyte is placed between the positive and negative electrodes, and fixed with tape to form a sandwich structure for sealing. Finally, the test frequency range is 0.1 to 10 6The AC impedance spectrum is tested under the condition of Hz, see Fig.18 ; In the voltage window of 0.8~1.9V, the current density is 0.91mA / cm 2 The constant current charge and discharge performance and cycle performance of the battery were tested under the condition of . The calculated ion conductivity of the cement-based diaphragm is 0.91S / m. The maximum specific capacity is 102.4mWh / g, and the energy decay is 6% after 1690 cycles.
Claims
1. A cement-based diaphragm, characterized in that: A number of etched pores are distributed on the cement-based diaphragm, which are obtained by etching away the components of the cement paste sheet with an acid solution, and the mass loss of the cement paste sheet is 5-40%; the cement paste sheet is further enlarged in porosity, pore size and pore connectivity through etching.
2. The cement-based diaphragm according to claim 1, characterized in that: The acidic solution is any one or a mixture of 1-5 mol / L ammonium chloride solution, 1-6 mol / L ammonium nitrate solution or 0.1-1 mol / L hydrochloric acid solution.
3. The cement-based diaphragm according to claim 1, characterized in that: The components of the etched cement paste slice include one or more of calcium silicate hydrate, calcium hydroxide, calcium carbonate, ettringite and the like.
4. A method for preparing the cement-based diaphragm according to claim 1, characterized in that: First, the cement paste slice is immersed in water and placed in a negative pressure environment to be fully saturated with water. Then, the saturated cement paste slice is immersed in an acidic solution to etch away the components of the cement paste. The mass loss of the cement paste slice is monitored. The etched cement paste slice is immersed in water to remove the etching solution, and then dried to obtain the cement-based diaphragm.
5. The method for preparing a cement-based diaphragm according to claim 4, characterized in that: The fully saturated water has a water immersion time of 1 to 3 days, and the negative pressure is -0.05 to -0.1 MPa.
6. The method for preparing the cement-based diaphragm according to claim 4, characterized in that: The cement slurry flakes are prepared with a water-cement ratio of 0.3 to 0.7, a stirring time of 60 to 90 seconds, a temperature of 18 to 22° C. in the curing room, a relative humidity of more than 95%, and an age of 1 to 180 days.
7. The method for preparing a cement-based diaphragm according to claim 4, characterized in that: The time for soaking the cement paste slice in water after etching is 1 to 7 days; the drying is one or more of natural drying, vacuum drying, freeze drying or microwave drying, and the drying time is 1 to 14 days.
8. An electrochemical energy storage device, characterized in that: The electrochemical energy storage device comprises the cement-based diaphragm according to any one of claims 1 to 3, two pole ears, a positive electrode and a negative electrode, wherein the pole ears are fixedly connected to the positive and negative electrodes respectively, and the cement-based diaphragm is immersed in the electrolyte under negative pressure and is placed between the positive and negative electrodes to form a sandwich structure.
9. The electrochemical energy storage device according to claim 8, characterized in that: The positive and negative electrodes are electrodes made of metal foil or active materials.
10. The electrochemical energy storage device according to claim 8, characterized in that: The specific method for preparing the active material electrode is as follows: firstly, the active material, the conductive agent and the binder are put into a mortar and ground evenly, then N-methylpyrrolidone is added and stirred rapidly, and finally the obtained slurry is evenly coated on a conductive carrier, and the active material electrode is obtained after drying.
Citation Information
Patent Citations
Novel structured supercapacitor taking graphene and cement as materials and fabrication of supercapacitor
CN105405676A
Diaphragms for electrolytic cells
GB1498733A
Diaphragm for electrolytic processes
GB207801A
Cited By
High-conductivity rechargeable cement-based battery and preparation method thereof
CN119560644A