Preparation method and application of double-layer composite nanofiber membrane moisture power generation device
The preparation of double-layer composite nanofiber membranes through electrospinning method solves the problems of cumbersome preparation process of moisture power generation devices and material structure design, improves moisture power generation efficiency and cycle stability, and achieves efficient moisture energy conversion.
Patent Information
- Application Number
- CN202410948746.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The preparation process of existing moisture power generation devices is cumbersome, with poor power generation efficiency and cycle stability. The moisture power generation devices prepared by a single material rely on external moisture, which limits their application scenarios and performance.
The double-layer composite nanofiber membrane was prepared by electrospinning. By doping cross-linked polymer solution and nanosilver, a double-layer nanofiber membrane with different hydrophilic group content was formed, which improved the response rate and cyclic stability.
It achieves efficient moisture adsorption and power generation performance improvement, avoids the problems of low power generation efficiency and poor cycle stability, and enhances the output voltage and antibacterial performance.
Smart Images

Figure CN118920913A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of wet gas power generation devices, and in particular to a preparation method and application of a double-layer composite nanofiber membrane wet gas power generation device. Background Art
[0002] As the global demand for energy continues to grow, people's attention to environmental protection and climate change is also increasing. The disadvantages of traditional power generation methods such as power generation with fossil fuels such as coal and oil are becoming more and more obvious, which has brought about problems such as global warming and resource depletion. Therefore, finding efficient and simple renewable resources is a way to alleviate the energy crisis and achieve sustainable development. Wet gas power generation, as a promising new energy conversion and collection technology, has attracted much attention. The main working mechanism of wet gas power generation is that after the functional material absorbs water molecules in the external environment, the ionized ions move in a directional manner to generate a potential difference and form a voltage.
[0003] At present, the preparation process of related wet gas power generation devices is relatively complicated and difficult to achieve large-scale production. At the same time, there are also problems with the structural design of power generation materials, which limits their power generation efficiency. For example: wet gas power generation devices made of a single material can only rely on the wet gas flow provided by the external environment to generate voltage, which limits the power generation efficiency and application scenarios; wet gas power generation devices without a large specific surface area will also reduce power generation efficiency and power generation due to the difficulty of water molecules entering.
[0004] The fiber membrane prepared by electrospinning technology has a large specific surface area and porosity. The wet gas power generation device prepared by this technology can quickly absorb moisture and generate voltage through ionization diffusion. By increasing the charge density, the power generation speed can be accelerated and the power generation can be increased. However, after multiple moisture absorption cycles, the fiber structure of the hydrophilic material becomes unstable and partially dissolves, resulting in reduced wet gas power generation performance and a shorter cycle period.
[0005] Therefore, using a simpler method to prepare a nanofiber membrane with a larger specific surface area and higher moisture absorption cycle stability is of great significance for the development of moisture power generation devices. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a preparation method and application of a double-layer composite nanofiber membrane moisture power generation device. Two cross-linked polymer solutions with different hydrophilic group contents are spun layer by layer through an electrospinning method to obtain a double-layer nanofiber membrane with different hydrophilic group concentrations. The membrane can quickly absorb moisture, has a faster response rate and higher current and voltage output, and has a more stable cycle performance, thus avoiding the problems of low power generation efficiency and power generation, as well as poor cycle stability of moisture power generation devices in the prior art.
[0007] In order to solve the above technical problems, the present invention provides a method for preparing a double-layer composite nanofiber membrane moisture power generation device, comprising the following steps:
[0008] S1, dissolving two portions of high molecular polymers containing hydrophilic groups in deionized water respectively, and then adding crosslinking agents respectively for crosslinking reaction to obtain crosslinked high molecular polymer solutions a and b having different hydrophilic group contents;
[0009] S2, adding nanosilver dispersion to the cross-linked polymer solutions a and b respectively, and mixing to obtain nanosilver-doped spinning solutions a and b;
[0010] S3, spinning the nanosilver-doped spinning solutions a and b layer by layer by electrospinning to obtain a double-layer nanofiber membrane with different hydrophilic group contents;
[0011] S4. Bond the side with higher hydrophilic group content in the double-layer nanofiber membrane to a perforated aluminum sheet as an upper electrode, and bond the side with lower hydrophilic group content to ITO conductive glass as a lower electrode. Connect the upper and lower electrodes with wires and fix them to obtain a double-layer composite nanofiber membrane moisture power generation device.
[0012] The nanofiber membrane prepared by the electrospinning method of the present invention has a high specific surface area and porosity, can achieve rapid adsorption and desorption of water molecules, and effectively improves the response rate of wet gas power generation. In addition, the high specific surface area increases the adsorption amount of water molecules and improves the power generation performance of the power generation device.
[0013] The present invention adopts a layer-by-layer spinning method to prepare a double-layer nanofiber membrane with different hydrophilic group contents. Compared with traditional gravity deposition, laser etching and other methods, the fiber membrane structure gradient can be controlled, and the nanofiber membranes with different hydrophilic group contents can be tightly combined, avoiding the ion diffusion and transmission obstacles caused by interlayer separation. At the same time, the double-layer nanofiber membrane with different hydrophilic group contents increases the ion concentration difference between the upper and lower electrodes after moisture absorption, thereby improving the output voltage of the device.
[0014] Furthermore, the cross-linked polymer solutions a and b satisfy at least one of the following conditions:
[0015] (1) using different types of the polymer containing hydrophilic groups;
[0016] (2) Adding different types and / or different amounts of the cross-linking agent.
[0017] The present invention achieves different hydrophilic group contents in the cross-linked polymer solutions a and b by changing the type of the polymer, the type of the cross-linking agent, the amount of the cross-linking agent added, or other methods.
[0018] Furthermore, the high molecular polymer containing a hydrophilic group is one or more of polyvinyl alcohol (PVA), polyethyleneimine (PEI), polyallylamine, sodium alginate (SA), and polyacrylic acid (PAA).
[0019] Furthermore, the total amount of polyvinyl alcohol, polyethyleneimine and polyallylamine added is 6%-9% of the mass of the spinning solution, and the total amount of sodium alginate and polyacrylic acid added is 0%-0.8% of the mass of the spinning solution.
[0020] Furthermore, the cross-linking agent is one or more of glutaraldehyde, boric acid, toluene diisocyanate, citric acid, and epichlorohydrin, and the added amount of the cross-linking agent is 1%-5% of the mass of the spinning solution.
[0021] Furthermore, the temperature of the cross-linking reaction is 50-80° C., and the reaction time is 3-6 hours.
[0022] The present invention realizes the cross-linking reaction by adding a cross-linking agent, and can more effectively control the cross-linking degree of the fiber membrane compared with the post-finishing method. Through the cross-linking between hydrophilic polymers, the structural collapse caused by the dissolution of nanofibers after moisture absorption is effectively avoided, thereby improving the hygroscopic power generation cycle stability of the composite nanofiber membrane, and realizing cyclic power generation under high humidity.
[0023] Furthermore, the particle size of the nanosilver is 5-50nm, and the amount of the nanosilver added is 30-100ppm of the spinning solution mass. Since the long-term moisture absorption cycle of the wet gas power generation device is prone to bacterial growth, the nanofiber membrane containing nanosilver is prepared by doping nanosilver, and silver ions are released during the moisture absorption process, which is not only conducive to increasing the amount of ion release and improving the power generation performance to a certain extent, but also can effectively inhibit bacterial growth, avoid the wet gas power generation device from being destroyed by microorganisms during use, and ensure its long-term stability.
[0024] Furthermore, the solvent of the nanosilver dispersion is water.
[0025] Furthermore, the electrospinning speed is 0.1-0.5 mL / h, the voltage is 17-20 kV, the receiving roller speed is 100-600 rpm / min, and the receiving distance is 15-20 cm.
[0026] Furthermore, the thickness of the nanofiber membrane with a higher hydrophilic group content in the double-layer nanofiber membrane is 60-80 μm, the thickness of the nanofiber membrane with a lower hydrophilic group content is 40-60 μm, and the thickness of the double-layer nanofiber membrane is 100-140 μm.
[0027] Furthermore, the antibacterial rate of the double-layer nanofiber membrane is above 99%, and it has excellent antibacterial properties.
[0028] Furthermore, the holes on the perforated aluminum sheet are evenly distributed, the hole diameter is 1-3 mm, and the total area of the holes accounts for 10%-20% of the total area of the aluminum sheet.
[0029] Furthermore, the fixing in S4 is specifically fixed by winding an insulating tape.
[0030] The second aspect of the present invention provides a double-layer composite nanofiber membrane moisture power generation device prepared by the preparation method described in the first aspect.
[0031] The third aspect of the present invention provides the application of the double-layer composite nanofiber membrane moisture power generation device described in the second aspect in the fields of moisture source monitoring, human breathing and movement monitoring, and conversion and collection of environmental moisture energy and electrical energy.
[0032] Furthermore, in the application, two or more of the double-layer composite nanofiber membrane moisture power generation devices are connected in series or in parallel. The two or more of the double-layer composite nanofiber membrane moisture power generation devices are connected in series or in parallel, which can meet the voltage and current requirements of the moisture power generation device in the application and have good cycle stability.
[0033] Beneficial effects of the present invention:
[0034] The present invention prepares cross-linked polymer solutions with different hydrophilic group contents by changing the type of polymer, the type or addition amount of the cross-linking agent, and then prepares double-layer nanofiber membranes with different hydrophilic group contents, thereby increasing the difference in ion concentration between the upper and lower electrodes after moisture absorption and improving the output voltage of the device.
[0035] The nanofiber membrane prepared by the electrospinning method in the present invention has a high specific surface area and porosity, can realize rapid adsorption and desorption of water molecules, effectively improve the response rate of wet gas power generation, and at the same time, effectively increase the adsorption amount of water molecules, and improve the power generation performance of the power generation device; through a layer-by-layer approach, the fiber membrane structure gradient can be controlled, and the nanofiber membrane layers with different hydrophilic group contents can be tightly combined, avoiding the ion diffusion and transmission barriers caused by interlayer separation.
[0036] The present invention adds a cross-linking agent to achieve a cross-linking reaction of the high molecular weight polymer, which can more effectively control the cross-linking degree of the fiber membrane compared to the post-finishing method; through the cross-linking between hydrophilic polymers, the structural collapse caused by the dissolution of the nanofibers after moisture absorption is effectively avoided, thereby improving the hygroscopic power generation cycle stability of the composite nanofiber membrane, and realizing cyclic power generation under high humidity.
[0037] The present invention prepares a nanofiber membrane containing nanosilver by doping nanosilver, and releases silver ions during moisture absorption, which is not only beneficial to increase the amount of ion release and improve power generation performance, but also can effectively inhibit bacterial growth, avoid moisture power generation devices being destroyed by microorganisms during use, and ensure their long-term stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a composition and structure model of the double-layer composite nanofiber membrane prepared in Examples 1, 2, and 3;
[0039] Figure 2 is a cross-sectional SEM image of the double-layer composite nanofiber membrane prepared in Example 1 and its element distribution map;
[0040] Figure 3 It is a single wet gas power generation performance test result diagram of the wet gas power generation devices prepared in Example 1 and Comparative Examples 1 and 2;
[0041] Figure 4 It is a comparison of the zeta potential of SA and PVA solutions;
[0042] Figure 5 1 is a graph showing the single wet gas power generation performance test results of the wet gas power generation devices prepared in Example 1 and Comparative Example 3;
[0043] Figure 6 is a schematic diagram of the wet gas generator of Example 1 and Comparative Example 3;
[0044] Figure 7 is a single wet gas power generation performance test result diagram of the wet gas power generation devices prepared in Examples 1, 2, and 3;
[0045] Figure 8 The multiple cycle wet gas power generation performance test graph and SEM graph of the wet gas power generation devices prepared in Example 1 and Comparative Example 4;
[0046] Fig. 9 It is a test diagram of wet gas power generation performance of wet gas power generation devices prepared in Example 1 and Comparative Example 5;
[0047] Fig.10 It is the application characterization of the wet gas power generation device prepared in Example 1 in human body signal monitoring and human body breathing monitoring;
[0048] Fig.11 Graphs showing open circuit voltage and short circuit current after connecting different numbers of wet gas power generation devices prepared in Example 1 in series and in parallel;
[0049] Fig.12 This is a diagram showing the application of 8 moisture power generation devices prepared in Example 1 connected in series as power generation devices to power LEDs. DETAILED DESCRIPTION
[0050] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0051] Example 1
[0052] This embodiment relates to a method for preparing a double-layer composite nanofiber membrane moisture power generation device, comprising the following steps:
[0053] S1. Preparation of spinning solution a: 0.7 g PVA and 0.06 g SA powder were dissolved in 8.04 g deionized water, and 0.2 g glutaraldehyde was added thereto. The mixture was heated and stirred at 60° C. for 4 h, and then 1 g of a nanosilver aqueous solution with an average particle size of 7.4 nm and a concentration of 500 ppm was added. The mixture was stirred and dispersed uniformly to obtain a cross-linked high molecular polymer spinning solution a with a PVA mass fraction of 7 wt%, a SA mass fraction of 0.6 wt%, a glutaraldehyde mass fraction of 2 wt%, and a nanosilver content of 50 ppm.
[0054] S2, preparation of spinning solution b: 0.7g PVA powder was dissolved in 8.1g deionized water, and 0.2g glutaraldehyde was added thereto, heated and stirred at 60°C for 4h, and then 1g of nanosilver aqueous solution with an average particle size of 7.4nm and a concentration of 500ppm was added, and stirred and dispersed evenly to obtain a cross-linked high molecular polymer spinning solution b with a PVA mass fraction of 7wt%, a glutaraldehyde mass fraction of 2wt%, and a nanosilver content of 50ppm.
[0055] S3, preparation of double-layer composite nanofiber membrane: First, the spinning solution a is loaded into the electrospinning equipment, and the electrospinning process parameters are set as spinning voltage of 18kV, spinning speed of 0.2mL / h, receiving distance of 18cm, and roller speed of 300rpm / min. By controlling the spinning time, a single-layer electrospun nanofiber membrane a with a thickness of 70μm is obtained. Then, the spinning solution b is replaced, and the spinning is continued with the same spinning process, and the nanofiber membrane a is continued to be collected. By controlling the spinning time, a nanofiber membrane b with a thickness of 50μm is obtained, and a double-layer composite nanofiber membrane with a total thickness of 120μm is obtained.
[0056] S4. Assembly of wet gas power generation device: Take 2cm×2cm aluminum sheet and ITO conductive glass as electrodes, punch 75 holes with a diameter of 1mm and a center spacing of 2mm evenly distributed on the aluminum sheet, and the hole area accounts for 14.7%. Cut the prepared double-layer composite nanofiber membrane into 2cm×2cm size, and then sandwich it between two electrodes made of aluminum sheet and ITO conductive glass. The side with a higher hydrophilic group content in the double-layer composite nanofiber membrane (fiber membrane a in this embodiment) is bonded to the punched aluminum sheet, and the side with a lower hydrophilic group content (fiber membrane b in this embodiment) is bonded to the conductive glass. At the same time, use conductive tape as a conductor and stick it to the inside of the electrode. Fix the assembled device with insulating tape to ensure effective contact between the material and the electrode to obtain a double-layer composite nanofiber membrane wet gas power generation device.
[0057] Example 2
[0058] The difference between this embodiment and embodiment 1 lies in the preparation of the spinning solution b, specifically: 0.7 g of PVA and 0.06 g of SA powder are dissolved in 7.94 g of deionized water, and then 0.3 g of glutaraldehyde is added thereto, heated and stirred at 60° C. for 4 h, and then 1 g of a nanosilver aqueous solution with an average particle size of 7.4 nm and a concentration of 500 ppm is added, and stirred and dispersed evenly to obtain a cross-linked high molecular polymer spinning solution b with a PVA mass fraction of 7 wt%, a SA mass fraction of 0.6 wt%, a glutaraldehyde mass fraction of 3 wt%, and a nanosilver content of 50 ppm.
[0059] Other parameters and steps are the same as those in Example 1.
[0060] Example 3
[0061] The difference between this embodiment and embodiment 2 lies in the preparation of the spinning solution b, specifically: 0.7 g of PVA and 0.06 g of SA powder are dissolved in 7.84 g of deionized water, and then 0.4 g of glutaraldehyde is added thereto, heated and stirred at 60° C. for 4 h, and then 1 g of a nanosilver aqueous solution with an average particle size of 7.4 nm and a concentration of 500 ppm is added, and stirred and dispersed evenly to obtain a cross-linked high molecular polymer spinning solution b with a PVA mass fraction of 7 wt%, a SA mass fraction of 0.6 wt%, a glutaraldehyde mass fraction of 4 wt%, and a nanosilver content of 50 ppm.
[0062] Other parameters and steps are the same as those in Example 2.
[0063] Example 4
[0064] The difference between this embodiment and embodiment 1 is that the concentration of the nanosilver aqueous solution added to the spinning solutions a and b is 300 ppm, and the cross-linked high molecular polymer spinning solutions a and b having a nanosilver content of 30 ppm are obtained.
[0065] Other parameters and steps are the same as those in Example 1.
[0066] Example 5
[0067] The difference between this embodiment and embodiment 1 is that the concentration of the nanosilver aqueous solution added to the spinning solutions a and b is 1000 ppm, and the cross-linked high molecular polymer spinning solutions a and b having a nanosilver content of 100 ppm are obtained.
[0068] Other parameters and steps are the same as those in Example 1.
[0069] Example 6
[0070] This embodiment relates to a method for preparing a double-layer composite nanofiber membrane moisture power generation device, comprising the following steps:
[0071] S1. Preparation of spinning solution a: 0.6 g PVA and 0.08 g PAA powder were dissolved in 8.12 g deionized water, and 0.2 g glutaraldehyde was added thereto. The mixture was heated and stirred at 50° C. for 6 h, and then 1 g of a nanosilver aqueous solution with an average particle size of 25 nm and a concentration of 400 ppm was added and stirred to disperse uniformly to obtain a cross-linked high molecular polymer spinning solution a with a PVA mass fraction of 6 wt%, a PAA mass fraction of 0.8 wt%, a glutaraldehyde mass fraction of 2 wt%, and a nanosilver content of 40 ppm.
[0072] S2, preparation of spinning solution b: 0.9g of polyallylamine powder was dissolved in 8g of deionized water, and then 0.1g of glutaraldehyde was added thereto, and the mixture was heated and stirred at 80°C for 4h, followed by adding 1g of a nanosilver aqueous solution with an average particle size of 25nm and a concentration of 400ppm, and stirred and dispersed evenly to obtain a cross-linked high molecular polymer spinning solution b with a polyallylamine mass fraction of 9wt%, a glutaraldehyde mass fraction of 1wt%, and a nanosilver content of 40ppm.
[0073] S3, preparation of double-layer composite nanofiber membrane: First, the spinning solution a is loaded into the electrospinning equipment, and the electrospinning process parameters are set as spinning voltage of 17kV, spinning speed of 0.3mL / h, receiving distance of 20cm, and roller speed of 600rpm / min. By controlling the spinning time, a single-layer electrospun nanofiber membrane a with a thickness of 80μm is obtained. Then, the spinning solution b is replaced, and the spinning is continued with the same spinning process, and the nanofiber membrane a is continued to be collected. By controlling the spinning time, a nanofiber membrane b with a thickness of 60μm is obtained, and a double-layer composite nanofiber membrane with a total thickness of 140μm is obtained.
[0074] S4. Assembly of wet gas power generation devices: Take 2cm×2cm aluminum sheets and ITO conductive glass as electrodes, punch 25 holes with a diameter of 2mm and a center spacing of 3mm evenly distributed on the aluminum sheet, and the hole area accounts for 20%. Cut the prepared double-layer composite nanofiber membrane into a size of 2cm×2cm, and then sandwich it between two electrodes made of aluminum sheets and ITO conductive glass. The side with a higher content of hydrophilic groups in the double-layer composite nanofiber membrane (fiber membrane a in this embodiment) is bonded to the punched aluminum sheet, and the side with a lower content of hydrophilic groups (fiber membrane b in this embodiment) is bonded to the conductive glass. At the same time, use conductive tape as a conductor and stick it to the inside of the electrode. Fix the assembled device with insulating tape to ensure effective contact between the material and the electrode.
[0075] Example 7
[0076] This embodiment relates to a method for preparing a double-layer composite nanofiber membrane moisture power generation device, comprising the following steps:
[0077] S1. Preparation of spinning solution a: 0.9 g PVA and 0.02 g SA powder are dissolved in 7.98 g deionized water, and then 0.1 g glutaraldehyde is added thereto. The mixture is heated and stirred at 80° C. for 3 h, and then 1 g of a nanosilver aqueous solution with an average particle size of 15 nm and a concentration of 300 ppm is added and stirred to disperse evenly to obtain a cross-linked high molecular polymer spinning solution a with a PVA mass fraction of 9 wt%, a SA mass fraction of 0.2 wt%, a glutaraldehyde mass fraction of 1 wt%, and a nanosilver content of 30 ppm.
[0078] S2, preparation of spinning solution b: 0.3g PVA and 0.5g PEI powder are dissolved in 8.1g deionized water, and then 0.1g glutaraldehyde is added thereto, and heated and stirred at 60°C for 4h, followed by adding 1g of nanosilver aqueous solution with an average particle size of 15nm and a concentration of 300ppm, and stirred and dispersed evenly to obtain a cross-linked high molecular polymer spinning solution b with a PVA mass fraction of 3wt%, a PEI mass fraction of 5wt%, a glutaraldehyde mass fraction of 1wt%, and a nanosilver content of 30ppm.
[0079] S3, preparation of double-layer composite nanofiber membrane: First, the spinning solution a is loaded into the electrospinning equipment, and the electrospinning process parameters are set as spinning voltage of 20kV, spinning speed of 0.1mL / h, receiving distance of 15cm, and roller speed of 100rpm / min. By controlling the spinning time, a single-layer electrospun nanofiber membrane a with a thickness of 60μm is obtained. Then, the spinning solution b is replaced, and the spinning is continued with the same spinning process, and the nanofiber membrane a is continued to be collected. By controlling the spinning time, a nanofiber membrane b with a thickness of 40μm is obtained, and a double-layer composite nanofiber membrane with a total thickness of 100μm is obtained.
[0080] S4. Assembly of wet gas power generation device: Take 2cm×2cm aluminum sheet and ITO conductive glass as electrodes, punch 9 holes with a diameter of 3mm and a center spacing of 5mm evenly distributed on the aluminum sheet, and the hole area accounts for 15.9%. Cut the prepared double-layer composite nanofiber membrane into a size of 2cm×2cm, and then sandwich it between two electrodes made of aluminum sheet and ITO conductive glass. The side with a higher hydrophilic group content in the double-layer composite nanofiber membrane (fiber membrane a in this embodiment) is bonded to the punched aluminum sheet, and the side with a lower hydrophilic group content (fiber membrane b in this embodiment) is bonded to the conductive glass. At the same time, use conductive tape as a conductor and stick it to the inside of the electrode. Fix the assembled device with insulating tape to ensure effective contact between the material and the electrode.
[0081] Comparative Example 1
[0082] The difference between this comparative example and Example 1 is that only spinning solution a is configured, and the spinning time is adjusted by the electrospinning process parameters of the single-layer electrospinning nanofiber membrane a in S3 to prepare a single-layer nanofiber membrane with a thickness of 120 μm, and the two sides of the single-layer nanofiber membrane are respectively bonded and fixed to an aluminum sheet and an ITO conductive glass by the method in S4 to obtain a single-layer nanofiber membrane moisture power generation device.
[0083] Other parameters and steps are the same as those in Example 1.
[0084] Comparative Example 2
[0085] The difference between this comparative example and Example 1 is that only spinning solution b is configured, and the spinning time is adjusted by the electrospinning process parameters of the single-layer electrospinning nanofiber membrane b in S3 to prepare a single-layer nanofiber membrane with a thickness of 120 μm, and the two sides of the single-layer nanofiber membrane are respectively bonded and fixed to an aluminum sheet and an ITO conductive glass by the method in S4 to obtain a single-layer nanofiber membrane moisture power generation device.
[0086] Other parameters and steps are the same as those in Example 1.
[0087] Comparative Example 3
[0088] The difference between this comparative example and Example 1 is that the side with higher hydrophilic group content in the double-layer composite nanofiber membrane (fiber membrane a in this comparative example) is bonded to the conductive glass, and the side with lower hydrophilic group content (fiber membrane b in this comparative example) is bonded to the perforated aluminum sheet.
[0089] Other parameters and steps are the same as those in Example 1.
[0090] Comparative Example 4
[0091] The difference between this comparative example and Example 1 is that no cross-linking agent is added to the spinning solution a and the spinning solution b, and the other parameters and steps are the same as those in Example 1.
[0092] Comparative Example 5
[0093] The difference between this comparative example and Example 1 is that no nanosilver is added to the spinning solution a and the spinning solution b, and the other parameters and steps are the same as those in Example 1.
[0094] Test Case
[0095] The raw materials and prepared nanofiber membranes in the above embodiments and comparative examples were tested and analyzed, and the assembled moisture power generation device was tested for the output effect of electrical signals. A UT61E+ multimeter was used to record all voltage signals in real time. The two heads were short-circuited before testing to ensure that the initial voltage was 0V. The test temperature was 25±1°C. The device was first placed in a balance dish filled with hygroscopic and color-changing silica gel and dried for 12 hours. During the test, it was transferred to an environment with a humidity of 85%, and the voltage or current generated by the device over time was recorded.
[0096] Figure 1 The composition structure model of the double-layer composite nanofiber membrane prepared in Examples 1, 2, and 3, wherein 2wt% G means adding 2% glutaraldehyde for cross-linking reaction, and the rest is analogous. It can be intuitively seen from the model that the three examples use different strategies to construct composite double-layer nanofiber membranes with different hydrophilic group contents. In Example 1, the spinning solution a increases the hydrophilic group content by adding SA, and Examples 2 and 3 adjust the cross-linking degree of the polymer in the upper and lower nanofiber membranes. In the spinning solution b, more glutaraldehyde is added, the cross-linking degree is high, and the hydrophilic group is relatively small.
[0097] Figure 2 The cross-sectional SEM image and element distribution diagram of the double-layer composite nanofiber membrane prepared in Example 1. It can be seen that the cross-sectional area of the double-layer composite nanofiber membrane prepared by layer-by-layer electrospinning does not show stratification, that is, the ion channels between the nanofiber membranes with different hydrophilic group contents remain intact when used for wet gas power generation. At the same time, the distribution diagram of the sodium element shows that it has an obvious double-layer structure, that is, the lower half of the picture is the nanofiber membrane layer containing sodium alginate.
[0098] Figure 3The results of a single wet gas power generation performance test of the wet gas power generation devices prepared in Example 1 and Comparative Examples 1 and 2 are shown. It can be seen that the output voltage of Example 1 is 0.412V, the output voltage of Comparative Example 1 is 0.383V, and the output voltage of Comparative Example 2 is only 0.308V. It can be seen that the output voltage of the wet gas power generation device assembled using only a single-layer structure nanofiber membrane (Comparative Examples 1 and 2) is significantly lower than that of the double-layer structure nanofiber membrane (Example 1), indicating that the double-layer differential structure can enhance the difference in ion concentration between electrodes, thereby increasing the potential difference between electrodes and increasing the output voltage. Moreover, compared with Comparative Examples 1 and 2, Example 1 has a faster response rate. In addition, the output voltage of Comparative Example 1 is higher than that of Comparative Example 2. This is because SA is added to Comparative Example 1 relative to Comparative Example 2. SA contains a large number of sodium carboxylate groups, which are easier to ionize sodium ions after moisture absorption, and have a larger negative potential after moisture absorption (reference Figure 4 ), thereby enhancing the potential difference between the electrodes, so the addition of SA is beneficial to improving the output voltage.
[0099] Figure 5 It is a test result diagram of the wet gas power generation performance of Example 1 and Comparative Example 3. The difference between the two is that in Comparative Example 3, when assembling the wet gas power generation device, the double-layer membrane was inverted, that is, the nanofiber membrane on the side without adding SA was bonded to the perforated aluminum sheet. From the results, it can be seen that when the wet gas power generation device (Example 1) with a higher content of hydrophilic groups is bonded to the perforated aluminum electrode, it has a larger voltage output and a faster response speed. However, the wet gas power generation device (Comparative Example 3) prepared in reverse has a slow response speed and a voltage output of only 0.181V. When the device with a positive gradient is exposed to a high humidity environment, the humid air flow enters the interior of the material from the upper electrode with holes, and the hydrophilic groups release ions by capturing water. Due to the asymmetric structure of the material, it has a concentration gradient of hydrophilic groups itself, forming a double concentration gradient structure. The ionized ions migrate from the high concentration area to the low concentration area with the diffusion of moisture, generating an open circuit voltage (such as Figure 6 As shown). After inversion, the hygroscopic side is a nanofiber membrane with a lower hydrophilic group concentration (without SA), which absorbs moisture slowly and has a low ion concentration. When moisture reaches the lower electrode area, this part of the nanofiber membrane is more likely to release ions, forming reverse diffusion, thereby reducing the difference in ion concentration and potential difference between the electrodes, so the output voltage is low. This shows that a reasonable double-layer structure is of great significance to improving device performance.
[0100] The wet gas power generation devices prepared in Examples 1, 2, and 3 were tested for single wet gas power generation performance. The results are shown in Figure 7It can be seen that the output voltages of Examples 2 and 3 are relatively close, but slightly lower than that of Example 1. This indicates that a double-layer composite nanofiber membrane with a differential structure can be constructed by material composition and different cross-linking degrees to ensure good voltage output. At the same time, the addition of a more hygroscopic and ionizable material can better construct a differential structure and improve device performance.
[0101] In order to meet the requirements of long-term use, the developed nanofiber membrane wet gas power generation device must have sufficient moisture absorption stability. Since the nanofiber membrane has a relatively thin diameter and the hydrophilic polymer is easy to absorb moisture, it is very easy to cause the structure to collapse after moisture absorption and cannot be recycled. Therefore, multiple cycles of wet gas power generation performance tests were conducted on Example 1 and Comparative Example 4. The results are shown in Table 1. Figure 8 Compared with Example 1, Comparative Example 4 did not add glutaraldehyde, that is, no cross-linking was performed. Figure 8 a and 8b, it can be seen that the voltage output performance of the uncrosslinked comparative example 4 decreased from 0.437V to 0.3521V after 3 cycles, a decrease of 19.42%; while the performance of the crosslinked example 1 was relatively stable after 10 cycles, with a decrease of only 3.24%. From the fiber structure before and after the cycle, it can be seen that the fiber morphology of the crosslinked example 1 changed less after 10 cycles ( Figure 8 c is the SEM image of the fiber membrane before moisture absorption cycle in Example 1, Figure 8 d is the SEM image of the fiber membrane after 10 moisture absorption cycles of Example 1), which proves that the addition of the crosslinking agent improves the structural stability of the nanofibers and can obtain better moisture cycle power generation performance. However, after 3 cycles of the uncrosslinked comparative example 4, the fibers are adhered to each other, the porosity is reduced, and the number of ion channels is reduced. ( Figure 8 e is the SEM image of the fiber membrane before moisture absorption cycle of comparative example 4, Figure 8 f is the SEM image of the fiber membrane after three moisture absorption cycles of comparative example 4), which is the reason for the decrease in output voltage.
[0102] Fig. 9 The wet gas power generation performance of Example 1 and Comparative Example 5 is compared. The difference between the two is that nanosilver is not added in Comparative Example 5. From the results, it can be seen that the power generation voltage of the device is slightly improved after the addition of nanosilver, indicating that the added nanosilver can release a certain amount of silver ions after the fiber absorbs moisture, and move in a directional manner with other cations to generate a higher output voltage. It proves that the addition of nanosilver can not only play an antibacterial role, but also improve the wet gas power generation performance to a certain extent.
[0103] The double-layer composite nanofiber membranes prepared in Examples 1, 4, 5 and Comparative Example 5 were subjected to antibacterial experiments on Escherichia coli and Staphylococcus aureus. The results are shown in Table 1. It can be seen from the table that Comparative Example 5 without the addition of nanosilver has no antibacterial property, while Examples 1, 4 and 5 all have excellent antibacterial properties, and the antibacterial rates can reach more than 99%.
[0104] Table 1
[0105]
[0106] Application Examples
[0107] The working mechanism of the moisture power generation device of the present invention is that the interaction between the external water molecules and the hygroscopic nanofiber membrane causes the transfer of ions inside the fiber membrane. When the external humidity is high, the nanofiber membrane absorbs more water and the voltage increases. Therefore, the voltage or current generated by the moisture power generation device can directly reflect the external humidity level. Therefore, it can be used as a monitoring device for moisture sources, such as monitoring human finger movements, breathing intensity, exercise intensity, etc.
[0108] Fig.10 a is a human body signal monitoring application. Using the moisture power generation device prepared in Example 1, place the finger above the side with holes on the device, and monitor different output voltages by changing the distance. As can be seen from the figure, the electrical signal changes with the change of the distance between the finger and the device. The finger itself carries sweat. When the distance increases, the moisture adsorbed by the device decreases, and the ionized ions decrease. For comparison, an ordinary pencil is placed above the device. No matter how the height is changed, the generation of electrical signals is not monitored. Therefore, using this point, the human body and other objects can be detected and distinguished. When the human body is close to the device, the voltage and current both increase to a certain extent, and it can also be used as an alarm monitoring device to serve as an alarm reminder.
[0109] In addition, the wet gas power generation device prepared in Example 1 was placed in a breathing device, such as a mask, and electrical signals with different waveforms and amplitudes were monitored by changing the breathing degree, such as Fig.10 As shown in Figure b. With the rhythm of breathing, the waveform of the output voltage signal is presented, and because deep breathing releases more water molecules than steady breathing, the signal is also significantly enhanced. Therefore, the device can be used to distinguish different breathing patterns and breathing rates, and monitor human breathing in real time. In the medical field, people with sleep apnea syndrome can be monitored in real time to ensure steady breathing during sleep. It can also be used in the sports field to monitor the breathing rate of athletes in real time.
[0110] In order to further improve the output performance of wet gas power generation devices and expand their application areas, the devices can be connected in series and in parallel to a certain number of times. Fig.11 The open circuit voltage and short circuit current of different numbers of sample devices in Example 1 are connected in series and parallel. A single device can generate an open circuit voltage of 0.41V and a short circuit current of 0.99μA. When the number of devices in series is 3 and 5, the open circuit voltage reaches 1.04V and 1.79V respectively, and the short circuit current has basically no change and is basically stable at 0.99μA. Fig.11a. When the number of parallel connections is 3 or 5, the open circuit voltage is almost stable at 0.41V, while the short circuit current is 0.97μA, 2.63μA, and 4.27μA respectively. Fig.11 b. It can be seen that the series and parallel connection of the power generation device basically meets the conclusion of the series-parallel law. The series and parallel connection of multiple devices can effectively improve the strength of the monitoring signal, and the output voltage can be effectively increased after series connection, which can be used as an energy collection and conversion device.
[0111] The eight wet gas power generation devices prepared in Example 1 were pressed Fig.12 A way to connect in series, the voltage can reach 2.8V after testing, using its moisture absorption to charge the capacitor (0.50F) for 2h, can light up a small LED bulb (see Fig.12 b).
[0112] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A method for preparing a double-layer composite nanofiber membrane wet gas power generation device, characterized in that: The steps include: S1, dissolving two portions of high molecular polymers containing hydrophilic groups in deionized water respectively, and then adding crosslinking agents respectively for crosslinking reaction to obtain crosslinked high molecular polymer solutions a and b having different hydrophilic group contents; S2, adding nanosilver dispersion to the cross-linked polymer solutions a and b respectively, and mixing to obtain nanosilver-doped spinning solutions a and b; S3, spinning the nanosilver-doped spinning solutions a and b layer by layer by electrospinning to obtain a double-layer nanofiber membrane with different hydrophilic group contents; S4. Bond the side with higher hydrophilic group content in the double-layer nanofiber membrane to a perforated aluminum sheet as an upper electrode, and bond the side with lower hydrophilic group content to ITO conductive glass as a lower electrode. Connect the upper and lower electrodes with wires and fix them to obtain a double-layer composite nanofiber membrane moisture power generation device.
2. The method for preparing the double-layer composite nanofiber membrane moisture power generation device according to claim 1, characterized in that: The cross-linked polymer solutions a and b satisfy at least one of the following conditions: (1) using different polymers containing hydrophilic groups; (2) Adding different types and / or different amounts of the cross-linking agent.
3. The method for preparing the double-layer composite nanofiber membrane moisture power generation device according to claim 1, characterized in that: The high molecular polymer containing a hydrophilic group is one or more of polyvinyl alcohol, polyethyleneimine, polyallylamine, sodium alginate, and polyacrylic acid.
4. The method for preparing the double-layer composite nanofiber membrane moisture power generation device according to claim 3, characterized in that: The total addition amount of the polyvinyl alcohol, polyethyleneimine and polyallylamine is 6%-9% of the mass of the spinning solution, and the total addition amount of the sodium alginate and polyacrylic acid is 0%-0.8% of the mass of the spinning solution.
5. The method for preparing the double-layer composite nanofiber membrane moisture power generation device according to claim 1, characterized in that: The cross-linking agent is one or more of glutaraldehyde, boric acid, toluene diisocyanate, citric acid and epichlorohydrin, and the added amount of the cross-linking agent is 1%-5% of the mass of the spinning solution.
6. The method for preparing the double-layer composite nanofiber membrane moisture power generation device according to claim 1, characterized in that: The particle size of the nano silver is 5-50 nm, and the added amount of the nano silver is 30-100 ppm of the spinning solution mass.
7. The method for preparing the double-layer composite nanofiber membrane moisture power generation device according to claim 1, characterized in that: The electrospinning speed is 0.1-0.5 mL / h, the voltage is 17-20 kV, the receiving roller speed is 100-600 rpm / min, and the receiving distance is 15-20 cm.
8. The method for preparing the double-layer composite nanofiber membrane moisture power generation device according to claim 1, characterized in that: The thickness of the nanofiber membrane of the layer with higher hydrophilic group content in the double-layer nanofiber membrane is 60-80 μm, and the thickness of the nanofiber membrane of the layer with lower hydrophilic group content is 40-60 μm.
9. A double-layer composite nanofiber membrane moisture power generation device prepared by the preparation method according to any one of claims 1 to 8.
10. An application of the double-layer composite nanofiber membrane moisture power generation device according to claim 9 in the fields of moisture source monitoring, human breathing and movement monitoring, and conversion and collection of environmental moisture energy and electrical energy.