All-inorganic perovskite battery with optimized hole transport layer and preparation method of all-inorganic perovskite battery

By adding 4,4'-disulfide bis[2,3,5,6-tetrafluoropyridine] to the hole transport layer of perovskite solar cells, the stability problem caused by Li-TFSI is solved and the conductance is improved rate and stability improve photoelectric conversion efficiency and long-term stability of devices.

CN118922038APending Publication Date: 2024-11-08SHAANXI NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975734.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The Li-TFSI additive in existing perovskite solar cells leads to poor air stability and thermal stability of the hole transport layer, and the diffusion of lithium ions leads to deterioration of interface performance, limiting the transmission process of photogenerated carriers and affecting the improvement of battery efficiency.

Method used

Doping in the hole transport layer using multifunctional organic additive 4,4'-disulfide bis[2,3,5,6-tetrafluoropyridine](2SF), accelerates the oxidation of Spiro-OMeTAD through the S-S bond, hinders Li+ The diffusion of ions reduces the surface charge recombination of the perovskite layer, improves the interface charge transfer efficiency, and enhances hydrophobicity through the C-F bond, inhibits the entry of moisture and oxygen in the air.

Benefits of technology

It significantly improves the conductivity and stability of the hole transport layer, improves the photoelectric conversion efficiency and working stability of all-inorganic perovskite batteries, and increases the photoelectric conversion efficiency from 19.26% to 21.95%, and is exposed to air for a long time. Maintain high efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922038A_ABST
    Figure CN118922038A_ABST
Patent Text Reader

Abstract

The invention discloses an all-inorganic perovskite battery with an optimized hole transport layer and a preparation method of the all-inorganic perovskite battery, and belongs to the technical field of perovskite materials. The inorganic perovskite C10F8N2S2 contains S-S, C-F and C = N bonds, and the bonds can effectively stabilize Li < + > ions in the hole transport layer through interaction and inhibit the Li < + > ions from migrating to the perovskite layer; besides, oxidation of Spiro-OMeTAD is accelerated by the oxidation performance of the S-S bond, the hole mobility and conductivity of the hole transport layer are improved, the photoelectric conversion efficiency of the all-inorganic CsPbI3 perovskite cell optimized by C10F8N2S2 is improved from 19.26% to 21.95%, and the all-inorganic CsPbI3 perovskite cell has excellent operation stability after optimization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of perovskite material and device preparation, and specifically relates to an all-inorganic perovskite battery with an optimized hole transport layer and a preparation method thereof. Background Art

[0002] Compared with the development and utilization of traditional fossil energy, clean solar energy started late but has developed rapidly. Driven by the relevant technologies of "carbon peak and carbon neutrality", how to efficiently develop and utilize solar energy has become the focus of people's attention.

[0003] Solar cells are devices that convert solar energy directly into electrical energy through the photoelectric conversion effect, and are an important way to develop and utilize solar energy in a green way. Among them, cells with perovskite semiconductor materials as light absorption layers (i.e., perovskite cells) are a new type of solar cell with advantages such as high light absorption efficiency, low binding force of photogenerated carriers, long carrier life and transmission distance, and low manufacturing cost. They are currently a new type of thin-film solar cell with great commercial prospects.

[0004] The cesium lead iodide (CsPbI3) perovskite light-absorbing layer constructed of all-inorganic components has excellent light and thermal stability and a suitable optical band gap (≈1.7eV), making it an ideal top cell material for building tandem solar cells. CsPbI3 perovskite cells based on traditional Spiro-OMeTAD hole transport materials have made extraordinary progress, with their photoelectric conversion efficiency (PCE) increasing from 3.8% at the beginning to 21.8%. Pure Spiro-OMeTAD films have low conductivity and require a long period of oxidation to produce high-conductivity Spiro + Ion radicals, thereby improving the charge conduction efficiency. Li-TFSI doping can greatly shorten the Spiro + The generation time of ion radicals is short, so Li-TFSI becomes a classic additive for Spiro-OMeTAD hole transport materials. However, Li-TFSI additives are highly hygroscopic and easily deteriorate when exposed to air, resulting in poor air stability and thermal stability of the hole transport material. At the same time, Li-TFSI dopants are easy to aggregate in the hole transport layer, and Li + Ions will also migrate to the perovskite layer, causing the interface performance of the hole transport layer / perovskite layer to deteriorate, seriously affecting the transport process of photogenerated carriers and limiting the improvement of the photovoltaic performance of the device. Therefore, the development of high-performance hole transport layer additives is crucial to improving battery efficiency and stability. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art and provide an all-inorganic perovskite battery with an optimized hole transport layer and a preparation method thereof, which solves the problem of poor stability caused by lithium ion diffusion in the hole transport layer by bulk doping of the hole transport layer.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing an all-inorganic perovskite cell with an optimized hole transport layer comprises the following steps:

[0008] S1, depositing an electron transport layer on the conductive glass, and preparing a CsPbI3 perovskite absorption layer on the electron transport layer;

[0009] S2, spin coating a Spiro-OMeTAD solution on the CsPbI3 perovskite absorption layer to prepare a hole transport layer; the preparation process of the Spiro-OMeTAD solution is as follows: dissolving Li-TFSI in acetonitrile to obtain a lithium salt solution, mixing the Spiro-OMeTAD powder, the lithium salt solution, t-BP and C 10 F8N2S2 were dissolved in chlorobenzene to obtain Spiro-OMeTAD solution; 10 The chemical structure of F8N2S2 is:

[0010]

[0011] S3, preparing a metal electrode on the hole transport layer.

[0012] A further improvement of the present invention is:

[0013] Preferably, in S2, the concentration of the lithium salt solution is 520 mg / mL.

[0014] Preferably, in S2, Spiro-OMeTAD powder, lithium salt solution, t-BP and C 10 The mixing ratio of F8N2S2 is 90mg:22μL:36μL:(0.5~4.0)mg.

[0015] Preferably, in S2, when spin coating the Spiro-OMeTAD solution, the spin coating speed is 5000 rpm and the spin coating time is 30 s.

[0016] Preferably, in S1, the electron transport layer is TiO2 or SnO2.

[0017] Preferably, in S1, the method for preparing the perovskite absorption layer is: spin coating a CsPbI3 perovskite precursor solution on the electron transport layer to prepare the CsPbI3 perovskite absorption layer.

[0018] Preferably, the concentration of the CsPbI3 perovskite precursor solution is 0.745M.

[0019] Preferably, the spin coating of the perovskite precursor solution is divided into two stages. In the first stage, the spin coating speed is 1000-1500 rpm and the spin coating time is 10 s; in the second stage, the spin coating speed is 3000-4000 rpm and the spin coating time is 40 s.

[0020] An all-inorganic perovskite cell with an optimized hole transport layer prepared by any of the above preparation methods, comprising a conductive glass, an electron transport layer, a CsPbI3 perovskite absorption layer, a hole transport layer and a metal electrode stacked in sequence from bottom to top;

[0021] The hole transport layer comprises Spiro-OMeTAD, lithium salt, t-BP and C 10 F8N2S2.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The invention discloses a method for preparing an all-inorganic perovskite with an optimized hole transport layer. The method comprises adding a multifunctional organic additive (4,4′-dithiobis[2,3,5,6-tetrafluoropyridine], C 10 F8N2S2], referred to as 2SF), uses the functional groups such as -SS-, CF, and pyridine ring in 2SF materials to improve the performance of the hole transport layer and the perovskite layer. The specific effects of this material are as follows: (1) The SS bond in 2SF can not only accelerate the oxidation of Spiro, but also help to obtain more Spiro + Free radicals increase the electrical conductivity of Spiro, and the SS bond and Li + The S-Li interaction and the C=N bond and Li + The C=N-Li interaction can effectively hinder the Li + Diffusion from the hole transport layer into the perovskite layer reduces the Li + (2) The fluorine-substituted pyridine ring in the 2SF at the interface can interact with the under-coordinated Pb on the surface of the inorganic perovskite film. 2+Through the interaction between F-Pb and C=N-Pb, the lead-related defects on the surface of the perovskite layer are effectively reduced, the recombination of surface charges is reduced, and the charge transfer efficiency at the interface is improved. (3) The doped 2SF material can reduce the conduction band and Fermi level of the hole transport layer, better achieve energy level matching with the perovskite layer, and thus reduce the hole transport barrier. (4) The presence of multiple CF bonds in 2SF enhances the hydrophobicity of the hole transport layer, which can effectively inhibit moisture and oxygen in the air from entering the perovskite layer, significantly improving the long-term storage and operation stability of the perovskite cell. This hole transport layer additive is applied to the preparation of different all-inorganic perovskite solar cells, which optimizes the film quality of the hole transport layer, reduces the holes on the surface of the hole transport layer, reduces the interface defects between the perovskite layer and the hole transport layer, and improves the photoelectric conversion efficiency and working stability of the all-inorganic perovskite cell.

[0024] The present invention discloses an all-inorganic perovskite battery with an optimized hole transport layer. The material contains SS, CF and C=N bonds, which interact with each other through chemical bonds and can effectively stabilize the Li in the hole transport layer. + ions, inhibiting Li + The ions migrate to the perovskite layer; in addition, the oxidation property of the SS bond accelerates the oxidation of Spiro-OMeTAD, and the hole mobility and conductivity of the hole transport layer are improved. The photoelectric conversion efficiency of the all-inorganic CsPbI3 perovskite cell optimized by 2SF is increased from 19.26% to 21.95%, and the optimized device has excellent operating stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 C 10 Fluorine spectrum of F8N2S2(2SF) by NMR;

[0026] Figure 2 C 10 Mass spectrum of F8N2S2(2SF);

[0027] Figure 3 This is a schematic diagram of the structure of the CsPbI3 perovskite solar cell described in Example 1 of the present invention;

[0028] Among them: 1 is FTO layer, 2 is electron transport layer, 3 is perovskite light absorption layer, 4 is hole transport layer (adding 2SF), and 5 is metal electrode;

[0029] Figure 4 This is the XPS spectrum of the interaction between 2SF and PbI2 described in Example 1 of the present invention;

[0030] Figure 5 This is a Fourier transform infrared spectrum of the reaction between 2SF and Li-TFSI described in Example 1 of the present invention;

[0031] Among them, (a) shows the FTIR (infrared) spectrum of CN of 2SF and Li-TFSI; (b) shows the FTIR (infrared) spectrum of SS of 2SF and Li-TFSI.

[0032] Figure 6 UPS comparison diagram of the hole transport layer (Spiro-OMeTAD) film without and with 2SF added as described in Example 1 of the present invention;

[0033] Figure 7 The JV curves of the perovskite solar cell without and with 2SF added as described in Example 1 of the present invention;

[0034] Figure 8 The stability of the perovskite solar cell without and with 2SF added as described in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] The present invention mainly develops a high-performance Spiro-OMeTAD hole transport material dopant 4,4′-disulfide bis[2,3,5,6-tetrafluoropyridine] (2SF) through chemical design and synthesis technology. 2SF contains SS, CF and C=N bonds, which can effectively stabilize the Li in the hole transport layer through the interaction of electronic electrostatic potential. + ions, inhibiting Li + ions migrate to the perovskite layer; in addition, the oxidation property of the SS bond accelerates the oxidation of Spiro-OMeTAD and improves the ability of the hole transport layer to conduct holes. The photoelectric conversion efficiency of the all-inorganic CsPbI3 perovskite cell optimized by 2SF has increased from 19.26% to 21.95%, and the optimized device can still maintain 96% of its initial efficiency after being exposed to air for 6000 hours of aging. In addition, the packaged device can still maintain 90% of its initial efficiency after continuous light aging for 1000 hours at the maximum output power point.

[0036] Preparation of 4,4′-dithiobis[2,3,5,6-tetrafluoropyridine]: Pentafluoropyridine (1.0 equiv., 14.6 mmol, 2.47 g) was added dropwise to a bottle containing aqueous sodium sulfide solution (2.5 equiv., 36.5 mmol, 2.71 g) and maintained below 30°C. The resulting solution was then stirred continuously for 20 minutes at 25°C and evaporated under reduced pressure. The residual solid was quenched with concentrated hydrochloric acid (40 mL) and then extracted with petroleum ether three times (1×70 mL and 2×35 mL). The combined organic phases were evaporated under reduced pressure and purified by column chromatography using ethyl acetate / hexane (1 / 6) as the eluent to obtain 2.57 g of 4,4′-dithiobis[2,3,5,6-tetrafluoropyridine] as a colorless liquid, which solidified at room temperature to obtain 4,4′-dithiobis[2,3,5,6-tetrafluoropyridine] as a solid.

[0037] Figure 1 C 10 The fluorine spectrum of F8N2S2 (2SF) in the NMR. There are two chemical environments of F in 2SF, so there are two peaks in the fluorine spectrum. Figure 2 C 10 The mass spectrum of F8N2S2(2SF), the relative molecular mass of 2SF is 367, Figure 1 and Figure 2 This indicates that C 10 F8N2S2.

[0038] The first aspect of the present invention discloses a method for preparing an all-inorganic perovskite battery, comprising the following steps:

[0039] Step 1, cleaning FTO glass;

[0040] Cut the FTO glass into 2.5×2.5cm 2 Clean the small pieces of glass with acetone, ethanol and isopropanol, then blow dry with an air compressor for later use.

[0041] Step 2: depositing an electron transport layer on the cleaned FTO glass, wherein the electron transport layer is TiO2 or SnO2.

[0042] The FTO glass cleaned in step 1 was treated with ultraviolet ozone for 10-15 minutes, and TiO2 was deposited by chemical deposition. 4.5 mL of TiCl4 was dropped on 200 mL of ice. After the ice melted to a certain size (about 1 cm × 4 cm), it was placed in a 70 ° C oven for deposition for 54 minutes, and then annealed. The thickness of the prepared TiO2 or SnO2 electron transport layer was 40-50 nm.

[0043] Step 3, prepare a perovskite precursor solution, wherein the perovskite precursor solution is a CsPbI3 perovskite precursor solution.

[0044] The process of preparing the CsPbI3 perovskite precursor solution is as follows: dissolve hydrogen lead iodine (HPbI3) and cesium iodide (CsI) (molar ratio = 0.745:0.825) in a mixed solvent of DMF and DMSO (V / V = 17:3) to prepare a CsPbI3 perovskite precursor solution with a concentration of 0.745M, stir the perovskite precursor solution for 8-12h, and then filter it using a 0.45μm syringe for later use.

[0045] Step 4, preparing a perovskite light absorbing layer;

[0046] The prepared perovskite precursor solution in step 3 is spin-coated on the surface of the FTO / TiO2 substrate. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000-1500rpm and the time is 10s; in the second stage, the rotation speed is 3000-4000rpm and the time is 40s. Then an annealing process is carried out, the annealing temperature is 170°C, and the annealing time is 50-55min. After annealing, a FTO / TiO2 / perovskite light-absorbing layer is formed. The prepared perovskite light-absorbing layer is 400-450nm.

[0047] Step 5, preparing a hole transport layer;

[0048] The hole transport layer is made of Spiro-OMeTAD. First, a lithium salt solution is prepared, and 520 mg of Li-TFSI solid is dissolved in 1 mL of acetonitrile to obtain a lithium salt solution. Then, Spiro-OMeTAD powder (90 mg), lithium salt solution (22 μL), t-BP (36 μL) and 0.5-4.0 mg of 2SF are dissolved in 1 mL of chlorobenzene to obtain a Spiro-OMeTAD solution. The Spiro-OMeTAD solution is spin-coated on the perovskite light-absorbing layer prepared in step 7 at a speed of 5000 rpm (acceleration of 3000 rpm / s) for 30 seconds to form a hole transport layer, and FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) is obtained.

[0049] The hole transport layer C 10 F8N2S2 is a multifunctional additive that can be directly added into the hole transport layer precursor solution to optimize the hole transport layer. The structural formula of the multifunctional additive is:

[0050]

[0051] The chemical formula of the hole transport layer additive material is: 10 F8N2S2 (2SF for short).

[0052] Step 6, preparing a metal electrode;

[0053] Gold with a thickness of about 40 nm is evaporated on the surface of the hole transport layer prepared in step 5 as a metal electrode to obtain an all-inorganic CsPbI3 perovskite solar cell with a structure of FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) / Au.

[0054] In a second aspect of the present invention, an all-inorganic CsPbI3 perovskite solar cell structure prepared by the above method is disclosed, see Figure 1 :

[0055] From bottom to top, it includes: FTO layer 1, TiO2 electron transport layer 2, CsPbI3 perovskite light absorption layer 3, Spiro-OMeTAD hole transport layer 4 and gold electrode 5.

[0056] Example 1

[0057] Step 1, cleaning FTO glass;

[0058] Cut the FTO glass into 2.5×2.5cm 2 Clean the small pieces of glass with acetone, ethanol and isopropanol, then blow dry with an air compressor for later use.

[0059] Step 2: depositing an electron transport layer on the cleaned FTO glass, wherein the electron transport layer is TiO2 or SnO2.

[0060] Treat the FTO glass washed in step 1 with ultraviolet ozone for 10-15 minutes. Deposit TiO2 by chemical deposition. Drop 4.5mL TiCl4 on 200mL ice, wait for the ice to melt to the size of a little finger, place in a 70℃ oven for 54 minutes, and then anneal. The thickness of the prepared TiO2 electron transport layer is 40-50nm.

[0061] Step 3, prepare a perovskite precursor solution, wherein the perovskite precursor solution is a CsPbI3 perovskite precursor solution.

[0062] The process of preparing the CsPbI3 perovskite precursor solution is as follows: dissolve hydrogen lead iodine (HPbI3) and cesium iodide (CsI) (molar ratio = 0.745:0.825) in a mixed solvent of DMF and DMSO (V / V = 17:3) to prepare a CsPbI3 perovskite precursor solution with a concentration of 0.745M, stir the perovskite precursor solution for 8-12h, and then filter it using a 0.45μm syringe for later use.

[0063] Step 4, preparing a perovskite light absorbing layer;

[0064] The prepared perovskite precursor solution in step 3 is spin-coated on the surface of the FTO / TiO2 substrate. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000-1500rpm and the time is 10s; in the second stage, the rotation speed is 3000-4000rpm and the time is 40s. Then an annealing process is carried out, the annealing temperature is 170°C, and the annealing time is 50-55min. After annealing, a FTO / TiO2 / perovskite light-absorbing layer is formed. The prepared perovskite light-absorbing layer is 400-450nm.

[0065] Step 5, preparing a hole transport layer;

[0066] The hole transport layer is made of Spiro-OMeTAD. First, a lithium salt solution is prepared, and 520 mg of Li-TFSI solid is dissolved in 1 mL of acetonitrile to obtain a lithium salt solution. Then, Spiro-OMeTAD powder (90 mg), lithium salt solution (22 μL), t-BP (36 μL) and 1 mg of 2SF are dissolved in 1 mL of chlorobenzene to obtain a 1 mg / mL 2SF Spiro-OMeTAD solution. The Spiro-OMeTAD solution is spin-coated on the perovskite light-absorbing layer prepared in step 7 at a speed of 5000 rpm (acceleration of 3000 rpm / s) for 30 seconds to form a hole transport layer, and FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) is obtained.

[0067] Step 6, preparing a metal electrode;

[0068] Gold with a thickness of about 40 nm is evaporated on the surface of the hole transport layer prepared in step 5 as a metal electrode to obtain an all-inorganic CsPbI3 perovskite solar cell with a structure of FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) / Au.

[0069] like Figure 3 As shown, it is a schematic diagram of the structure of an all-inorganic CsPbI3 perovskite solar cell, in which: 1 is FTO, 2 is a TiO2 electron transport layer, 3 is a CsPbI3 perovskite light absorption layer, 4 is a Spiro-OMeTAD hole transport layer (with 2SF added), and 5 is a gold electrode. Among them, the concentration of 2SF added is 1 mg / mL.

[0070] like Figure 4 As shown in the figure, the interaction between 2SF and PbI2 is explained. As can be seen from the figure, Pb moves towards the direction of low binding energy, which indicates that 2SF and the under-coordinated Pb in PbI2 2+ Combined to fill Pb 2+ And you can see that the unadded Pb 2+ There is zero-valent lead, which disappears after addition.

[0071] like Figure 5 As shown in the figure, the interaction between 2SF and Li-TFSI is explained. As can be seen from the figure, the characteristic peaks of CN and SS have obvious shifts. These bonds interact through electronic electrostatic potential and can effectively stabilize the Li in the hole transport layer. + ions, inhibiting Li + The ions migrate to the perovskite layer.

[0072] like Figure 6As shown in the figure, after adding 2SF, the hole transport layer has a lower conduction band and Fermi level, which is beneficial to the extraction of holes and reduces the transfer barrier, resulting in an increase in the open circuit voltage of the device.

[0073] like Figure 7 As shown in Figure 2, the open circuit voltage and fill factor of the all-inorganic perovskite solar cell with 2SF addition are improved, which are 1.287V open circuit voltage and 81.92% fill factor, respectively, and the device efficiency is 21.95%, 20.80mA / cm 2 The current density is 21.95% and the photoelectric conversion efficiency is 21.95%.

[0074] like Figure 8 As shown, the stability of the film after addition was tested, and the optimal device can maintain 95% of the initial efficiency after 6000 hours, with good stability.

[0075] Comparative Example 1

[0076] The comparative example 1 is different from the embodiment 1 only in step 5. In step 5, 2SF is not added in the comparative example 1. The other steps and parameters are the same.

[0077] Figure 6 This is a UPS comparison chart of the hole transport layer (Spiro-OMeTAD) film without and with 2SF added. It can be seen that after adding 2SF, the Spiro-OMeTAD film has a lower conduction band and Fermi level. The perovskite film with the addition of 2SF is also more compatible with the hole transport layer, which increases the open circuit voltage of the device.

[0078] Figure 7 The JV curves of the all-inorganic CsPbI3 perovskite solar cells without and with the hole transport layer (Spiro-OMeTAD) film of 2SF are shown in Table 1. It can be seen that compared with the control sample without 2SF, the fill factor and open circuit voltage of the device after adding 2SF are improved, with the highest values ​​of 1.287V and 81.92%, and the efficiency of the best device prepared is 21.95%.

[0079] Figure 8 The stability of the efficiency of the device without and with 2SF added is shown under an air temperature of 25°C and a humidity of about 15-20%. After 6000 hours, the optimized sample can still maintain 96% of the initial efficiency.

[0080] Example 2

[0081] In this embodiment, 2SF is not added to the hole transport layer, and the rest remains unchanged. After washing the FTO glass and depositing titanium oxide by chemical deposition, the prepared CsPbI3 perovskite precursor solution is spin-coated on the surface of the FTO / TiO2 substrate. The spin coating process is divided into two stages. In the first stage, the rotation speed is 1000 rpm and the time is 10s; in the second stage, the rotation speed is 3000 rpm and the time is 40s. Subsequently, an annealing process is carried out with an annealing temperature of 170°C and an annealing time of 50min. The prepared hole transport layer precursor solution is spin-coated on the surface of FTO / TiO2 / perovskite. The all-inorganic CsPbI3 perovskite solar cell prepared on the substrate surface obtained an open circuit voltage of 1.220V, a fill factor of 77.32%, and a 2 The current density and the photoelectric conversion efficiency of 19.26% are the same as those in Example 1. Figure 5 .

[0082] Example 3

[0083] In this embodiment, the concentration of 2SF added to the hole transport layer is 0.5 mg / mL, and the remaining steps are the same as in Example 1. In this example, the efficiency of the inorganic perovskite solar cell is 20.96%.

[0084] Example 4

[0085] In this embodiment, the concentration of 2SF added to the hole transport layer is 2 mg / mL, and the remaining steps are the same as in Example 1. In this example, the efficiency of the inorganic perovskite solar cell is 21.09%.

[0086] Example 5

[0087] In this embodiment, the concentration of 2SF added to the hole transport layer is 3 mg / mL, and the remaining steps are the same as in Example 1. In this example, the efficiency of the inorganic perovskite solar cell is 21.02%.

[0088] Example 6

[0089] In this embodiment, the concentration of 2SF added to the hole transport layer is 4 mg / mL, and the remaining steps are the same as in Example 1. In this example, the efficiency of the inorganic perovskite solar cell is 20.38%.

[0090] Example 7

[0091] Step 1, cleaning FTO glass;

[0092] Cut the FTO glass into 2.5×2.5cm 2 Clean the small pieces of glass with acetone, ethanol and isopropanol, then blow dry with an air compressor for later use.

[0093] Step 2: depositing an electron transport layer on the cleaned FTO glass, wherein the electron transport layer is TiO2 or SnO2.

[0094] Treat the FTO glass washed in step 1 with ultraviolet ozone for 10-15 minutes. Deposit TiO2 by chemical deposition. Drop 4.5mL TiCl4 on 200mL ice, wait for the ice to melt to the size of a little finger, place in a 70℃ oven for 54 minutes, and then anneal. The thickness of the prepared TiO2 electron transport layer is 40-50nm.

[0095] Step 3, prepare a perovskite precursor solution, wherein the perovskite precursor solution is a CsPbI3 perovskite precursor solution.

[0096] The process of preparing the CsPbI3 perovskite precursor solution is as follows: Hydrogen lead iodine (HPbI3), cesium iodide (CsI) and hydrogen lead bromine (HPbBr3) (molar ratio = 0.723:0.825:0.022) are dissolved in a mixed solvent of DMF and DMSO (V / V = 17:3) to prepare a CsPbI3 solution with a concentration of 0.745 M. x Br 3-x Perovskite precursor solution: The perovskite precursor solution was stirred for 8-12 h and then filtered using a 0.45 μm syringe for later use.

[0097] Step 4, preparing a perovskite light absorbing layer;

[0098] The prepared perovskite precursor solution in step 3 is spin-coated on the surface of the FTO / TiO2 substrate. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000-1500rpm and the time is 10s; in the second stage, the rotation speed is 3000-4000rpm and the time is 40s. Then an annealing process is carried out, the annealing temperature is 170°C, and the annealing time is 50-55min. After annealing, a FTO / TiO2 / perovskite light-absorbing layer is formed. The prepared perovskite light-absorbing layer is 400-450nm.

[0099] Step 5, preparing a hole transport layer;

[0100] The hole transport layer was prepared using Spiro-OMeTAD. First, a lithium salt solution was prepared, and 520 mg of Li-TFSI solid was dissolved in 1 mL of acetonitrile to obtain a lithium salt solution. Then, Spiro-OMeTAD powder (90 mg), lithium salt solution (22 μL), t-BP (36 μL) and 1 mg of 2SF were dissolved in 1 mL of chlorobenzene to obtain a Spiro-OMeTAD solution. The Spiro-OMeTAD solution was spin-coated on the perovskite light-absorbing layer prepared in step 7 at a speed of 5000 rpm (acceleration of 3000 rpm / s) for 30 seconds to form a hole transport layer to obtain FTO / TiO2 / CsPbI x Br 3-x / Spiro-OMeTAD (added with 2SF).

[0101] Step 6, preparing a metal electrode;

[0102] Gold with a thickness of about 40 nm was evaporated on the surface of the hole transport layer prepared in step 5 as a metal electrode to obtain a structure of FTO / TiO2 / CsPbI x Br 3-x All-inorganic CsPbI / Spiro-OMeTAD (with 2SF) / Au x Br 3-x Perovskite solar cells.

[0103] Example 8

[0104] Step 1, cleaning FTO glass;

[0105] Cut the FTO glass into small pieces of 2.5×2.5 cm, clean them with acetone, ethanol and isopropanol, and blow dry them with an air compressor for later use.

[0106] Step 2: depositing an electron transport layer on the cleaned FTO glass, wherein the electron transport layer is TiO2 or SnO2.

[0107] Treat the FTO glass washed in step 1 with ultraviolet ozone for 10-15 minutes. Deposit TiO2 by chemical deposition. Drop 4.5mL TiCl4 on 200mL ice, wait for the ice to melt to the size of a little finger, place in a 70℃ oven for 54 minutes, and then anneal. The thickness of the prepared TiO2 electron transport layer is 40-50nm.

[0108] Step 3: Prepare a perovskite precursor solution, the perovskite precursor solution is CsPbI x Br 3-x Perovskite precursor solution.

[0109] The process of preparing the CsPbI3 perovskite precursor solution is as follows: Hydrogen lead iodine (HPbI3), cesium iodide (CsI) and hydrogen lead bromide (HPbBr3) (molar ratio = 0.730:0.825:0.015) are dissolved in a mixed solvent of DMF and DMSO (V / V = 17:3) to prepare a CsPbI3 solution with a concentration of 0.745 M. x Br 3-x Perovskite precursor solution: The perovskite precursor solution was stirred for 8-12 h and then filtered using a 0.45 μm syringe for later use.

[0110] Step 4, preparing a perovskite light absorbing layer;

[0111] The prepared perovskite precursor solution in step 3 is spin-coated on the surface of the FTO / TiO2 substrate. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000-1500rpm and the time is 10s; in the second stage, the rotation speed is 3000-4000rpm and the time is 40s. Then an annealing process is carried out, the annealing temperature is 170°C, and the annealing time is 50-55min. After annealing, a FTO / TiO2 / perovskite light-absorbing layer is formed. The prepared perovskite light-absorbing layer is 400-450nm.

[0112] Step 5, preparing a hole transport layer;

[0113] The hole transport layer was prepared using Spiro-OMeTAD. First, a lithium salt solution was prepared, and 520 mg of Li-TFSI solid was dissolved in 1 mL of acetonitrile to obtain a lithium salt solution. Then, Spiro-OMeTAD powder (90 mg), lithium salt solution (22 μL), t-BP (36 μL) and 1 mg of 2SF were dissolved in 1 mL of chlorobenzene to obtain a Spiro-OMeTAD solution. The Spiro-OMeTAD solution was spin-coated on the perovskite light-absorbing layer prepared in step 7 at a speed of 5000 rpm (acceleration of 3000 rpm / s) for 30 seconds to form a hole transport layer to obtain FTO / TiO2 / CsPbI x Br 3-x / Spiro-OMeTAD (added with 2SF).

[0114] Step 6, preparing a metal electrode;

[0115] Gold with a thickness of about 40 nm was evaporated on the surface of the hole transport layer prepared in step 5 as a metal electrode to obtain a structure of FTO / TiO2 / CsPbI x Br 3-x All-inorganic CsPbI / Spiro-OMeTAD (with 2SF) / Au x Br 3-x Perovskite solar cells.

[0116] Example 9

[0117] Step 1, cleaning FTO glass;

[0118] Cut the FTO glass into small pieces of 2.5×2.5 cm, clean them with acetone, ethanol and isopropanol, and blow dry them with an air compressor for later use.

[0119] Step 2: depositing an electron transport layer on the cleaned FTO glass, wherein the electron transport layer is TiO2 or SnO2.

[0120] Treat the FTO glass washed in step 1 with ultraviolet ozone for 10-15 minutes. Deposit TiO2 by chemical deposition. Drop 4.5mL TiCl4 on 200mL ice, wait for the ice to melt to the size of a little finger, place in a 70℃ oven for 54 minutes, and then anneal. The thickness of the prepared TiO2 electron transport layer is 40-50nm.

[0121] Step 3: Prepare a perovskite precursor solution, the perovskite precursor solution is CsPbI x Br 3-x Perovskite precursor solution.

[0122] Preparation of CsPbI x Br 3-x The process of perovskite precursor solution is as follows: Hydrogen lead iodine (HPbI3), cesium iodide (CsI) and hydrogen lead bromide (HPbBr3) (molar ratio = 0.738:0.825:0.007) are dissolved in a mixed solvent of DMF and DMSO (V / V = 17:3) to prepare CsPbI3 with a concentration of 0.745M. x Br 3-x Perovskite precursor solution: The perovskite precursor solution was stirred for 8-12 h and then filtered using a 0.45 μm syringe for later use.

[0123] Step 4, preparing a perovskite light absorbing layer;

[0124] The prepared perovskite precursor solution in step 3 is spin-coated on the surface of the FTO / TiO2 substrate. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000-1500rpm and the time is 10s; in the second stage, the rotation speed is 3000-4000rpm and the time is 40s. Then an annealing process is carried out, the annealing temperature is 170°C, and the annealing time is 50-55min. After annealing, a FTO / TiO2 / perovskite light-absorbing layer is formed. The prepared perovskite light-absorbing layer is 400-450nm.

[0125] Step 5, preparing a hole transport layer;

[0126] The hole transport layer was prepared using Spiro-OMeTAD. First, a lithium salt solution was prepared, and 520 mg of Li-TFSI solid was dissolved in 1 mL of acetonitrile to obtain a lithium salt solution. Then, Spiro-OMeTAD powder (90 mg), lithium salt solution (22 μL), t-BP (36 μL) and 1 mg of 2SF were dissolved in 1 mL of chlorobenzene to obtain a Spiro-OMeTAD solution. The Spiro-OMeTAD solution was spin-coated on the perovskite light-absorbing layer prepared in step 7 at a speed of 5000 rpm (acceleration of 3000 rpm / s) for 30 seconds to form a hole transport layer to obtain FTO / TiO2 / CsPbI x Br 3-x / Spiro-OMeTAD (added with 2SF).

[0127] Step 6, preparing a metal electrode;

[0128] Gold with a thickness of about 40 nm was evaporated on the surface of the hole transport layer prepared in step 5 as a metal electrode to obtain a structure of FTO / TiO2 / CsPbI x Br 3-x All-inorganic CsPbI / Spiro-OMeTAD (with 2SF) / Au x Br 3-x Perovskite solar cells.

[0129] Example 10

[0130] In this embodiment, the concentration of 2SF added to the hole transport layer is 0.5 mg / mL, and the remaining steps are the same as in Example 7.

[0131] Embodiment 11

[0132] In this embodiment, the concentration of 2SF added to the hole transport layer is 2 mg / mL, and the remaining steps are the same as in Example 7.

[0133] Example 12

[0134] In this embodiment, the concentration of 2SF added to the hole transport layer is 0.5 mg / mL, and the remaining steps are the same as in Example 8.

[0135] Embodiment 13

[0136] In this embodiment, the concentration of 2SF added to the hole transport layer is 2 mg / mL, and the remaining steps are the same as in Example 8.

[0137] Embodiment 14

[0138] In this embodiment, the concentration of 2SF added to the hole transport layer is 0.5 mg / mL, and the remaining steps are the same as in Example 9.

[0139] Embodiment 15

[0140] In this embodiment, the concentration of 2SF added to the hole transport layer is 2 mg / mL, and the remaining steps are the same as in Example 9.

[0141] Example 16

[0142] Step 1, cleaning FTO glass;

[0143] Cut the FTO glass into small pieces of 2.5×2.5 cm, clean them with acetone, ethanol and isopropanol, and blow dry them with an air compressor for later use.

[0144] Step 2: depositing an electron transport layer on the cleaned FTO glass, wherein the electron transport layer is TiO2 or SnO2.

[0145] Treat the FTO glass washed in step 1 with ultraviolet ozone for 10-15 minutes. Deposit TiO2 by chemical deposition. Drop 4.5mL TiCl4 on 200mL ice, wait for the ice to melt to the size of a little finger, place in a 70℃ oven for 54 minutes, and then anneal. The thickness of the prepared TiO2 electron transport layer is 40-50nm.

[0146] Step 3, prepare a perovskite precursor solution, wherein the perovskite precursor solution is a CsPbI3 perovskite precursor solution.

[0147] The process of preparing the CsPbI3 perovskite precursor solution is as follows: dissolve hydrogen lead iodine (HPbI3), cesium iodide (CsI) and cesium chloride (CsCl) (molar ratio = 0.745:0.825:0.029) in a mixed solvent of DMF and DMSO (V / V = 17:3) to prepare a CsPbI3 perovskite precursor solution with a concentration of 0.745M, stir the perovskite precursor solution for 8-12h, and then filter it using a 0.45μm syringe for later use.

[0148] Step 4, preparing a perovskite light absorbing layer;

[0149] The prepared perovskite precursor solution in step 3 is spin-coated on the surface of the FTO / TiO2 substrate. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000-1500rpm and the time is 10s; in the second stage, the rotation speed is 3000-4000rpm and the time is 40s. Then an annealing process is carried out, the annealing temperature is 170°C, and the annealing time is 50-55min. After annealing, a FTO / TiO2 / perovskite light-absorbing layer is formed. The prepared perovskite light-absorbing layer is 400-450nm.

[0150] Step 5, preparing a hole transport layer;

[0151] The hole transport layer is made of Spiro-OMeTAD. First, a lithium salt solution is prepared, and 520 mg of Li-TFSI solid is dissolved in 1 mL of acetonitrile to obtain a lithium salt solution. Then, Spiro-OMeTAD powder (90 mg), lithium salt solution (22 μL), t-BP (36 μL) and 1 mg of 2SF are dissolved in 1 mL of chlorobenzene to obtain a Spiro-OMeTAD solution. The Spiro-OMeTAD solution is spin-coated on the perovskite light-absorbing layer prepared in step 7 at a speed of 5000 rpm (acceleration of 3000 rpm / s) for 30 seconds to form a hole transport layer, and FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) is obtained.

[0152] Step 6, preparing a metal electrode;

[0153] Gold with a thickness of about 40 nm is evaporated on the surface of the hole transport layer prepared in step 5 as a metal electrode to obtain an all-inorganic CsPbI3 perovskite solar cell with a structure of FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) / Au.

[0154] Embodiment 17

[0155] Step 1, cleaning FTO glass;

[0156] Cut the FTO glass into small pieces of 2.5×2.5 cm, clean them with acetone, ethanol and isopropanol, and blow dry them with an air compressor for later use.

[0157] Step 2: depositing an electron transport layer on the cleaned FTO glass, wherein the electron transport layer is TiO2 or SnO2.

[0158] Treat the FTO glass washed in step 1 with ultraviolet ozone for 10-15 minutes. Deposit TiO2 by chemical deposition. Drop 4.5mL TiCl4 on 200mL ice, wait for the ice to melt to the size of a little finger, place in a 70℃ oven for 54 minutes, and then anneal. The thickness of the prepared TiO2 electron transport layer is 40-50nm.

[0159] Step 3, prepare a perovskite precursor solution, wherein the perovskite precursor solution is a CsPbI3 perovskite precursor solution.

[0160] The process of preparing the CsPbI3 perovskite precursor solution is as follows: dissolve hydrogen lead iodide (HPbI3), cesium iodide (CsI) and cesium bromide (CsBr) (molar ratio = 0.745:0.825:0.023) in a mixed solvent of DMF and DMSO (V / V = 17:3) to prepare a CsPbI3 perovskite precursor solution with a concentration of 0.745M, stir the perovskite precursor solution for 8-12h, and then filter it using a 0.45μm syringe for later use.

[0161] Step 4, preparing a perovskite light absorbing layer;

[0162] The prepared perovskite precursor solution in step 3 is spin-coated on the surface of the FTO / TiO2 substrate. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000-1500rpm and the time is 10s; in the second stage, the rotation speed is 3000-4000rpm and the time is 40s. Then an annealing process is carried out, the annealing temperature is 170°C, and the annealing time is 50-55min. After annealing, a FTO / TiO2 / perovskite light-absorbing layer is formed. The prepared perovskite light-absorbing layer is 400-450nm.

[0163] Step 5, preparing a hole transport layer;

[0164] The hole transport layer is made of Spiro-OMeTAD. First, a lithium salt solution is prepared, and 520 mg of Li-TFSI solid is dissolved in 1 mL of acetonitrile to obtain a lithium salt solution. Then, Spiro-OMeTAD powder (90 mg), lithium salt solution (22 μL), t-BP (36 μL) and 1 mg of 2SF are dissolved in 1 mL of chlorobenzene to obtain a Spiro-OMeTAD solution. The Spiro-OMeTAD solution is spin-coated on the perovskite light-absorbing layer prepared in step 7 at a speed of 5000 rpm (acceleration of 3000 rpm / s) for 30 seconds to form a hole transport layer, and FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) is obtained.

[0165] Step 6, preparing a metal electrode;

[0166] Gold with a thickness of about 40 nm is evaporated on the surface of the hole transport layer prepared in step 5 as a metal electrode to obtain an all-inorganic CsPbI3 perovskite solar cell with a structure of FTO / TiO2 / CsPbI3 / Spiro-OMeTAD (with 2SF added) / Au.

[0167] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

[0168] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an all-inorganic perovskite battery with an optimized hole transport layer, characterized in that: The following steps are involved: S1, depositing an electron transport layer on the conductive glass, and preparing a CsPbI3 perovskite absorption layer on the electron transport layer; S2, spin coating Spiro-OMeTAD solution on the CsPbI3 perovskite absorption layer to prepare a hole transport layer; The preparation process of the Spiro-OMeTAD solution is as follows: dissolving Li-TFSI in acetonitrile to obtain a lithium salt solution, mixing Spiro-OMeTAD powder, the lithium salt solution, t-BP and C 10 F8N2S2 were dissolved in chlorobenzene to obtain Spiro-OMeTAD solution; 10 The chemical structure of F8N2S2 is: S3, preparing a metal electrode on the hole transport layer.

2. The method for preparing an all-inorganic perovskite battery with an optimized hole transport layer according to claim 1, characterized in that: In S2, the concentration of the lithium salt solution is 520 mg / mL.

3. The method for preparing an all-inorganic perovskite battery with an optimized hole transport layer according to claim 1, characterized in that: In S2, Spiro-OMeTAD powder, lithium salt solution, t-BP and C 10 The mixing ratio of F8N2S2 is 90mg:22μL:36μL:(0.5~4.0)mg.

4. The method for preparing an all-inorganic perovskite battery with an optimized hole transport layer according to claim 1, characterized in that: In S2, when the Spiro-OMeTAD solution is spin-coated, the spin-coating speed is 5000 rpm and the spin-coating time is 30 s.

5. The method for preparing an all-inorganic perovskite battery with an optimized hole transport layer according to claim 1, characterized in that: In S1, the electron transport layer is TiO2 or SnO2.

6. The method for preparing an all-inorganic perovskite battery with an optimized hole transport layer according to claim 1, characterized in that: In S1, the method for preparing the perovskite absorption layer is: spin coating a CsPbI3 perovskite precursor solution on the electron transport layer to prepare the CsPbI3 perovskite absorption layer.

7. The method for preparing an all-inorganic perovskite battery with an optimized hole transport layer according to claim 6, characterized in that: The concentration of the CsPbI3 perovskite precursor solution is 0.745M.

8. The method for preparing an all-inorganic perovskite battery with an optimized hole transport layer according to claim 6, characterized in that: The spin coating of the perovskite precursor solution is divided into two stages. In the first stage, the spin coating speed is 1000-1500 rpm and the spin coating time is 10 s; in the second stage, the spin coating speed is 3000-4000 rpm and the spin coating time is 40 s.

9. An all-inorganic perovskite battery with an optimized hole transport layer prepared by any one of the preparation methods of claims 1-8, characterized in that: It includes conductive glass, electron transport layer, CsPbI3 perovskite absorption layer, hole transport layer and metal electrode stacked in sequence from bottom to top; The hole transport layer comprises Spiro-OMeTAD, lithium salt, t-BP and C 10 F8N2S2.