Syndiotactic polystyrene low dielectric sheet molded body

By using a styrene-based polymer with a gauge structure and an appropriate amount of fibrous filler in the sheet molded body, combined with a non-fibrous filler, the problem of large dimensional change rate and the problem of reduced dielectric characteristics after bidirectional stretching is solved, and the problem of reducing dielectric characteristics is achieved. Excellent performance and low cost production of high-frequency circuit substrates.

CN118922491APending Publication Date: 2024-11-08TOYOBO CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380029229.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the film after bidirectional stretching has a large dimensional change rate at high temperature, and the dielectric characteristics of the laminated body containing glass cloth have deteriorated, making it difficult to be applied to high-frequency circuit substrates, and the equipment investment is high and the cost is unreasonable.

Method used

Using a non-stretched sheet molded body, containing a styrene-based polymer, a fibrous filler and a non-fibrous filler with a syngastic structure, the composition and treatment conditions of the composition can be optimized to achieve low linear expansion coefficient and low thermal shrinkage. , improve welding heat resistance and dielectric characteristics.

Benefits of technology

It provides excellent signal speed and dimensional stability at high temperatures on high-frequency circuit substrates, reduces equipment investment and cost, while avoiding the problem of large dimensional change rate and dielectric characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052647240000211
    Figure BDA0005052647240000211
  • Figure BDA0005052647240000221
    Figure BDA0005052647240000221
  • Figure BDA0005052647240000222
    Figure BDA0005052647240000222
Patent Text Reader

Abstract

Provided is a sheet molded body having excellent dielectric properties and welding heat resistance, and further exhibiting a low dimensional change rate (low thermal shrinkage) and a low linear expansion coefficient. A sheet molded body containing a styrene polymer (A) having a syndiotactic structure, a fibrous filler (C), and a non-fibrous filler (D), the fibrous filler (C) is contained in an amount of 1 to 50 parts by mass per 100 parts by mass of the styrene polymer (A) having the syndiotactic structure, and the relative permittivity of the sheet molded article in the frequency band of 10 GHz is 3 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a non-stretched sheet molded body containing a syndiotactic polystyrene polymer having excellent dielectric properties, and more particularly to a non-stretched sheet molded body containing a syndiotactic polystyrene polymer, having excellent welding heat resistance, low thermal shrinkage and low linear expansion. Background Art

[0002] In recent years, the development of high-speed information communication materials and applications such as 5G has been booming. In order to increase the transmission speed of information, a plastic material with a low dielectric constant and dielectric loss tangent in the high-frequency band above 10GHz is sought. Among them, syndiotactic polystyrene (SPS) resin has excellent dielectric properties, so it is expected to be widely used in printed circuit boards and flexible printed circuit boards, etc., for circuit boards that require high-frequency characteristics.

[0003] Such circuit boards are often exposed to high temperature environments during use / manufacturing processes, and generally require high heat resistance / dimensional stability. The heat resistance referred to here refers to the property of being able to withstand the heat treatment conditions (e.g., 260°C, about 120 seconds) in the soldering process during the manufacturing stage of circuit boards and electronic components.

[0004] Patent Document 1 discloses a method for producing a release film made of a biaxially oriented plastic film treated at a predetermined heat treatment temperature after biaxially stretching a film containing 80% by weight or more of a syndiotactic polystyrene resin. Patent Document 2 discloses a laminate for a printed wiring board obtained by laminating 1 to 95% by weight of a glass cloth surface-treated with a coupling agent to 99 to 5% by weight of a forming material for a printed wiring board made of a styrene polymer having a highly syndiotactic structure containing a polar group. Prior art literature Patent Literature

[0005] Patent Document 1: Japanese Patent No. 5896753 Patent Document 2: Japanese Patent Publication No. 7-142830 Summary of the invention Problem that the invention aims to solve

[0006] However, as described in Patent Document 1, the equipment investment required for the stretching / heat treatment for biaxial stretching is huge, and it is difficult to cope with the cost requirements required for film making. In addition, although the film itself is oriented and crystallized by stretching to improve the characteristics, since the strain during stretching cannot be completely relieved, when the film is heated again at high temperature, there is a problem of large dimensional change rate. Therefore, it is difficult to apply in applications such as circuit substrates that require high dimensional stability. The laminate with glass cloth described in Patent Document 2 contains a large amount of polar group-modified SPS and a large amount of glass cloth with significantly deteriorated dielectric properties, so it is difficult to apply to high-frequency circuit substrates. In addition, there are problems with the thickness unevenness in the in-plane direction of the sheet and the adhesion of the interface with the glass cloth, which is a low practical solution.

[0007] In view of the above circumstances, an object of the present invention is to provide a sheet molded product which is excellent in dielectric properties and soldering heat resistance and further exhibits a low dimensional change rate (low thermal shrinkage) and a low linear expansion coefficient. Technical means of solving problems

[0008] The present inventors have made intensive studies to solve the above problems and have achieved the present invention. That is, the present invention is a sheet formed article as described below.

[0009] [1] A sheet-like formed article comprising a styrene-based polymer (A) having a syndiotactic structure, a fibrous filler (C) and a non-fibrous filler (D), The sheet material formed body is a non-stretched sheet material formed body, The fibrous filler (C) is contained in an amount of 1 to 50 parts by mass relative to 100 parts by mass of the styrene polymer (A) having a syndiotactic structure, The sheet formed body has a relative dielectric constant of 3 or less in a frequency band of 10 GHz. [2] The sheet molded product according to [1], comprising 1 to 40 parts by mass of a rubber-like elastic body (B) based on 100 parts by mass of the styrene polymer (A) having a syndiotactic structure. [3] The sheet material according to [1] or [2], wherein the fibrous filler (C) is glass fiber having a D50 average fiber length of 40 to 4000 μm. [4] The sheet material according to any one of [1] to [3], wherein the non-fibrous filler (D) is a granular or spherical filler having a D50 average particle size of 0.1 to 45 μm. [5] The sheet formed article according to any one of [1] to [4], wherein the rubber-like elastic body (B) contains a styrene-based or olefin-based thermoplastic elastomer. [6] A sheet forming body according to any one of [1] to [5], wherein the coefficient of linear expansion in the longitudinal direction (MD) and the transverse direction (TD) of the sheet forming body is 10 to 80 ppm / °C, and the ratio of MD / TD is in the range of 0.6 to 1.4. [7] The sheet formed article according to any one of [1] to [6], wherein the absolute value of the dimensional change rate of the sheet formed article after heat treatment at 150°C for 30 minutes is less than 0.4%. Effects of the Invention

[0010] The sheet forming body of the present invention has excellent dielectric properties and soldering heat resistance, and further exhibits low dimensional change rate (low thermal shrinkage) and low linear expansion coefficient. Therefore, it is possible to provide an excellent sheet forming body that can meet the signal speed required by high-frequency circuit substrates and dimensional stability at high temperatures. DETAILED DESCRIPTION

[0011] <Styrene polymer having a syndiotactic structure (A)> In the present invention, the syndiotactic structure in the styrene-based polymer having a syndiotactic structure as the component (A) (hereinafter also referred to as "SPS" or "syndiotactic polystyrene" or component (A)) means that the stereochemical structure is a syndiotactic structure, that is, a stereo structure having phenyl groups as side chains alternately and in opposite directions on the main chain formed by carbon-carbon bonds, and its stereoregularity is determined by carbon isotope nuclear magnetic resonance (C-NMR). The stereoregularity measured by the C-NMR method can be expressed by the existence ratio of multiple continuous structural units, for example, in the case of 2, it is represented by a diad, in the case of 3, it is represented by a triad, and in the case of 5, it is represented by a pentad. The styrene polymer with a syndiotactic structure in the present invention refers to: polystyrene, poly(alkyl styrene), poly(halogenated styrene), poly(halogenated alkyl styrene), poly(alkoxy styrene), poly(vinyl benzoate), their hydrogenated polymers and mixtures thereof or copolymers with them as the main components having a syndiotactic diad preferably 75 mol% or more, more preferably 85 mol% or more, or in the case of syndiotactic pentad preferably 30 mol% or more, more preferably 50 mol% or more.

[0012] It should be noted that the poly(alkylstyrene) herein includes poly(methylstyrene), poly(ethylstyrene), poly(isopropylstyrene), poly(tert-butylstyrene), poly(phenylstyrene), poly(vinylnaphthalene), poly(vinylstyrene), etc.; the poly(halogenated styrene) includes poly(chlorostyrene), poly(bromostyrene), poly(fluorostyrene), etc. In addition, the poly(halogenated alkylstyrene) includes poly(chloromethylstyrene), etc., and the poly(alkoxystyrene) includes poly(methoxystyrene), poly(ethoxystyrene), etc.

[0013] Among these, particularly preferred styrene polymers include polystyrene, poly(p-methylstyrene), poly(m-methylstyrene), poly(p-tert-butylstyrene), poly(p-chlorostyrene), poly(m-chlorostyrene), poly(p-fluorostyrene), hydrogenated polystyrene, and copolymers containing structural units thereof.

[0014] The styrene polymer (A) with a syndiotactic structure can be a copolymer of styrene with a syndiotactic structure and other monomers. The content of styrene with a syndiotactic structure in the (A) component is preferably 50% by mass or more. More preferably 60% by mass or more, further preferably 70% by mass or more, further preferably 80% by mass or more, particularly preferably 90% by mass or more, and most preferably 100% by mass. By making the content of styrene with a syndiotactic structure be 50% by mass or more, dielectric properties, welding heat resistance, dimensional change rate and linear expansion coefficient are excellent. In particular, since the above-mentioned performance degradation may occur, the content of the unsaturated nitrile group-containing monomer is preferably low, specifically preferably 2 mass % or less, more preferably less than 2 mass %, further preferably 1 mass % or less, and particularly preferably 0 mass %.

[0015] The styrene polymer (A) having a syndiotactic structure can be used by mixing one or more styrene polymers. There is no particular restriction on the composition ratio of the styrene copolymer, but the content of the substituted styrene unit is preferably in the range of 3 to 50 mol%. The modification can be easily performed if the content is 3 mol% or more, and compatibility with other components can be maintained if the content is 50 mol% or less.

[0016] There is no particular restriction on the molecular weight of the styrene polymer (A) having a syndiotactic structure, preferably a weight average molecular weight of 10,000 or more, more preferably 50,000 or more, and more preferably 100,000 or more. Further, there is no restriction on the width of the molecular weight distribution, and various (A) components can be used. By making the weight average molecular weight of 10,000 or more, the thermal properties and mechanical properties of the obtained composition or molded product are not reduced, and a good molded product is obtained. The upper limit is not particularly limited, preferably 500,000 or less, more preferably 400,000 or less.

[0017] For example, in an inert hydrocarbon solvent or in the absence of a solvent, a styrene-based polymer (A) having a syndiotactic structure can be produced by polymerizing a styrene-based monomer (a monomer corresponding to the above-mentioned styrene-based polymer) using a titanium compound and a condensation product of water and trialkylaluminum as a catalyst (Japanese Patent Publication No. 62-187708). In addition, poly(halogenated alkylstyrene) can be produced by Japanese Patent Publication No. 1-46912, and their hydrogenated polymers can be produced by the method described in Japanese Patent Publication No. 1-178505.

[0018] The melt flow rate (MFR) of the styrene polymer (A) having a syndiotactic structure measured at a temperature of 300° C. and a load of 1.2 kg is preferably 1 to 60 g / 10 minutes, more preferably 2 to 40 g / 10 minutes, further preferably 3 to 30 g / 10 minutes, and most preferably 4 to 20 g / 10 minutes. By setting the melt flow rate within the above range, a sheet having good physical properties can be obtained, and the film thickness of the sheet can be made uniform.

[0019] Representative commercial products of the syndiotactic structured styrene polymer (A) used in the present invention include, for example, XAREC (registered trademark) 142ZE, XAREC (registered trademark) 300ZC, XAREC (registered trademark) 130ZC, and XAREC (registered trademark) 90ZC manufactured by Idemitsu Kosan Co., Ltd. Among these resins, one type may be used alone, or two or more types may be mixed and used.

[0020] The styrene polymer (A) having a syndiotactic structure may not be modified by a compound containing a polar group (hereinafter also referred to as an unmodified (A) component), or may be modified (hereinafter also referred to as a modified (A) component). As the (A) component, it may be a single unmodified (A) component, a single modified (A) component, or a mixed component of an unmodified (A) component and a modified (A) component. Preferably, it is a single unmodified (A) component or a mixed component of an unmodified (A) component and a modified (A) component, and more preferably, it is a single unmodified (A) component. The content of the (A) component in the sheet forming body is the total amount of the unmodified (A) component and the modified (A) component. The modification amount in the modified (A) component is preferably greater than 0.01% by mass, more preferably greater than 0.1% by mass, and further preferably greater than 1.0% by mass. By modifying the styrene polymer (A) having a syndiotactic structure within the above range, the affinity of the unmodified component (A) with the fibrous filler (C) and the non-fibrous filler (D) is improved.

[0021] As the mixing amount of the modified (A) component, it is expected that it is preferably in the range of 0.01 to 40% by mass, more preferably in the range of 0.05 to 30% by mass relative to the total amount of the (A) component. By making this content more than 0.01% by mass, the effect as a compatibilizer can be exerted. In addition, it is not necessary to contain a large amount of modified (A) components, and the mechanical properties and heat resistance of the composition are not negatively affected. In addition, by making this content less than 40% by mass, the dielectric properties can be prevented from decreasing.

[0022] The compound containing the polar group is not particularly limited, but includes maleic acid, phthalic acid, glycidyl (meth)acrylate, and their anhydrides or esters and amines, etc. As the modified (A) component, for example, maleic anhydride-modified SPS, fumaric acid-modified SPS, glycidyl methacrylate-modified SPS, amine-modified SPS, etc. can be mentioned.

[0023] <Rubber-like elastic body (B)> When the sheet is wound, the rubbery elastic body (B) (hereinafter also referred to as component (B)) is preferably mixed because it can suppress the rupture of the sheet by improving the mechanical properties while imparting appropriate flexibility. The rubbery elastic body (B) component may include a single polymer composed of polyolefin, polystyrene or polyacrylate or a composition composed of a plurality of copolymers containing these components. Specific examples of the rubber-like elastomer include natural rubber, polybutadiene, polyisoprene, polyisobutylene, chloroprene rubber, polysulfide rubber, polysulfide rubber, acrylic rubber, polyurethane rubber, silicone rubber, epichlorohydrin rubber, ethylene-propylene copolymer rubber (EPM), ethylene-propylene-diene copolymer rubber (EPDM), ethylene-α-olefin copolymer rubber, styrene-butadiene block copolymer (SBR), hydrogenated styrene-butadiene block copolymer (SEB, SEBC), styrene-butadiene-styrene block copolymer (SBS), hydrogenated styrene-butadiene-styrene block copolymer (SEBS), styrene-isoprene block copolymer (SIR), hydrogenated styrene-isoprene block copolymer (SBR), hydrogenated styrene-butadiene block copolymer (SEB, SEBC), styrene-butadiene-styrene block copolymer (SBS), hydrogenated styrene-butadiene-styrene block copolymer (SEBS), styrene-isoprene block copolymer (SIR), hydrogenated styrene-isoprene block copolymer (S Core-shell type granular elastomers include styrene-isoprene-styrene block copolymer (SIS), hydrogenated styrene-isoprene-styrene block copolymer (SEPS), butadiene-acrylonitrile-styrene core-shell rubber (ABS), methyl methacrylate-butadiene-styrene core-shell rubber (MBS), methyl methacrylate-butyl acrylate-styrene core-shell rubber (MAS), octyl acrylate-butadiene-styrene core-shell rubber (MABS), alkyl acrylate-butadiene-acrylonitrile-styrene core-shell rubber (AABS), butadiene-styrene core-shell rubber (SBR), methyl methacrylate-butyl acrylate-siloxane-based core-shell rubber and other siloxane-containing core-shell rubbers or rubbers modified thereof.

[0024] Among these, SEBS, SIR, SEP, SIS, SEPS, ethylene-α-olefin copolymer rubber or their modified rubber are particularly preferably used. In addition, these rubber-like elastomers can be used alone as only one, or two or more can be used in combination. From the viewpoint of the processing temperature when mixed with the styrene polymer (A) having a syndiotactic structure, a rubber-like elastomer with high heat resistance is preferred. By mixing the rubber-like elastomer with partially selective hydrogenation of unsaturated bonds or fully hydrogenated, the gas generated during hot pressing can be suppressed, and even if exposed to a high temperature environment, the mechanical properties of the sheet forming body can be maintained.

[0025] The melt flow rate (MFR) of the rubbery elastic body (B) measured at a temperature of 230°C and a load of 2.16 kg is preferably 0.1 to 40 g / 10 min, more preferably 1.0 to 20 g / 10 min, and still more preferably 1.5 to 14 g / 10 min. By making the melt flow rate within the above range, the compatibility with the styrene polymer (A) having a syndiotactic structure can be improved, and the film thickness of the sheet can be made uniform.

[0026] When containing a rubber-like elastomer (B), its content is preferably 1 to 40 parts by mass relative to 100 parts by mass of the styrene copolymer (A) having a syndiotactic structure. More preferably, it is 3 to 30 parts by mass, and further preferably, it is 5 to 25 parts by mass. By making the content of component (B) more than 1 part by mass, the flexibility of the sheet forming body is improved, and the winding property on the roller is good. In addition, the hole opening processability in the subsequent drilling process is improved. In addition, by making the content of component (B) less than 40 parts by mass, it is possible to suppress the sheet forming body from being too soft, prevent adhesion on the roller, and maintain the heat resistance required for the high-frequency circuit substrate.

[0027] The rubber-like elastic body (B) preferably contains a styrene-based thermoplastic elastomer. When the rubber-like elastic body (B) is a styrene-based thermoplastic elastomer, the styrene content is preferably 5 to 60% by mass. More preferably 8 to 50% by mass, further preferably 10 to 40% by mass, and particularly preferably 15 to 32% by mass. By making the styrene content more than 5% by mass, the compatibility of (A) component and (B) component is improved, and the mechanical properties are good. In addition, by making the styrene content less than 60% by mass, the elastic modulus of (B) component will not be too high, so the effect of stress relaxation is improved, so when the flexibility of the sheet forming body becomes good, the polarity of the sheet forming body is suppressed, and the rise of the dielectric constant is suppressed.

[0028] <Fibrous filler (C)> The fibrous filler (C) (hereinafter also referred to as component (C)) is a fibrous filler that can improve the linear expansion coefficient of the sheet molded body in the direction parallel to the extrusion direction (MD) and the effect of suppressing dimensional change, and is a filler required for the sheet molded body of the present invention that has a lot of residual strain although it is not stretched. The fibrous filler (C) can use inorganic fibers or organic fibers. In the case of inorganic fibers, wollastonite (or whisker) or glass fiber can be used, and glass fiber is particularly preferred in view of dielectric properties. In order to achieve the desired balance between linear expansion coefficient and dimensional stability and impact resistance / mechanical properties, the content of fibrous filler (C) is 1 to 50 parts by mass relative to 100 parts by mass of styrene polymer (A) having a syndiotactic structure. Preferably, it is 3 to 40 parts by mass, and more preferably, it is 5 to 30 parts by mass.

[0029] The fibrous filler (C) may be in the form of roving, surface mats, chopped strand mat, satin fabric, plaid fabric, plain fabric, mesh plain fabric, twill fabric, net, or the like, and may be in the form of glass containing a large amount of alkali (C glass), alkali-free glass (E glass), or the like.

[0030] More preferably, it is glass containing more boric acid (D glass) or glass in which the balance of silicate and boric acid is adjusted (NE glass). In D glass, SiO2 and B2O3 are preferably contained, and the preferred range of SiO2 content is 65.0 to 80.0 mass%, and the preferred range of B2O3 content is 15.0 to 30.0 mass%. In NE glass, SiO2 and B2O3 are preferably contained, and the preferred range of SiO2 content is 45.0 to 65.0 mass%, and the preferred range of B2O3 content is 10.0 to 25.0 mass%.

[0031] Glass fibers with circular or non-circular cross-sections can be used as fibrous fillers (C). Glass fibers with non-circular cross-sections may be roughly elliptical, roughly oblong, or roughly cocoon-shaped in the cross-section perpendicular to the length of the fiber, and the flatness at this time is preferably 1.5 to 8. The flatness here refers to the ratio of the long diameter to the short diameter when a rectangle of the minimum area circumscribed to a cross-section perpendicular to the length of the glass fiber is assumed, with the length of the long side of the rectangle being the long diameter and the length of the short side being the short diameter. The thickness of the glass fiber is not particularly limited, and the short diameter is about 1 to 20 μm and the long diameter is about 2 to 100 μm. As glass fibers with circular cross-sections, the diameter of the fiber diameter is preferably 1 to 50 μm, more preferably 2 to 20 μm, and further preferably 3 to 15 μm.

[0032] The D50 average fiber length of the fibrous filler (C) is preferably 40 μm to 4000 μm, more preferably 40 μm to 3200 μm, further preferably 45 μm to 2000 μm, and most preferably 50 μm to 500 μm. When the D50 average fiber length is 40 μm or more, the surface area of ​​the fibrous filler (C) is large enough, the interface adhesion between the (A) component and the (C) component as the matrix resin is improved, and the physical properties of the sheet forming body are good. In addition, by making the D50 average fiber length 4000 μm or less, it is possible to suppress the excessive rigidity of the sheet forming body during film making and suppress the generation of cracks observed during the winding of the sheet. It is further possible to suppress the generation of agglomerates in the sheet forming body.

[0033] The fibrous filler (C) may or may not be surface treated. When the fibrous filler (C) is surface treated, examples of coupling agents used for the surface treatment include silane coupling agents and titanium coupling agents. Among them, from the viewpoint of compatibility with component (A), it is particularly preferred to use a silane coupling agent for surface treatment. Specific examples of silane coupling agents include: triethoxysilane, vinyl tris(β-methoxyethoxy)silane, γ-methacryloxypropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, β-(1,1-epoxycyclohexyl)ethyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl methyldimethoxysilane, γ-aminopropyl triethoxysilane, N-phenyl-γ-aminopropyl trimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyl-tri(2-methoxy-ethoxy)silane, N-methyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, 3-4,5-dihydroimidazolepropyltriethoxysilane, hexamethyldisilazane, N,N-bis(trimethylsilyl)urea, 3-triethoxysilyl-N-(1,3-dimethyl-butenyl)propylamine, etc. Among these, aminosilanes and epoxysilanes such as γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane are preferred.

[0034] Specific examples of titanium coupling agents include triisostearoyl isopropyl titanate, tri(dodecylbenzenesulfonyl) isopropyl titanate, tri(dioctyl pyrophosphoryl) isopropyl titanate, bis(dioctyl phosphite) tetraisopropyl titanate, bis(ditridecylphosphite) tetraoctyl titanate, tetrakis(1,1-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphoryl) Oxyacetyl titanate, bis(dioctyl pyrophosphoryl)ethylene titanate, trioctanoyl isopropyl titanate, dimethacryloyl isostearyl titanate isopropyl, isostearyl diacryloyl titanate isopropyl, tri(dioctylphosphoryl) titanate isopropyl, triisopropylphenyl phenyl titanate isopropyl, tri(N-amidoethyl, aminoethyl) titanate isopropyl, phenyloxyacetyl diisopropylphenyl titanate, diisostearoyl ethylene titanate, etc. Among these, tri(N-amidoethyl, aminoethyl) titanate isopropyl is preferred.

[0035] There is no particular restriction on the surface treatment method of the fibrous filler (C) using the coupling agent. For example, it can be carried out by applying a sizing treatment using an organic solvent solution or suspension of the coupling agent as a sizing agent to the fibrous filler (C), dry mixing treatment using a Henschel mixer, a super mixer, a Loedige mixer, a V-type blender, etc., by a spray method, an overall blending method, a dry concentration method, etc., which are suitable for the shape of the fibrous filler (C). Among them, it is preferred to carry out the surface treatment by sizing treatment, dry mixing treatment, and spraying. It is possible to use a film-forming substance for glass, for example, while using the coupling agent. There is no particular restriction on the film-forming substance, and examples thereof include: polyester, urethane, epoxy, acrylic, vinyl acetate, polyether and other polymers.

[0036] As a compatibilizer for the fibrous filler (C), in addition to the styrene polymer (A) having a syndiotactic structure, a modified polymer can also be used. By adding a compatibilizer, the syndiotactic polystyrene polymer (A) can be mixed with the fibrous filler (C) and the non-fibrous filler (D) for the purpose of improving the interface strength.

[0037] Specific examples of the compatibilizer include: styrene-maleic anhydride copolymer (SMA), styrene-glycidyl methacrylate copolymer, terminal carboxylic acid-modified polystyrene, terminal epoxy-modified polystyrene, terminal oxazoline-modified polystyrene, terminal amine-modified polystyrene, sulfonated polystyrene, styrene-based ionomers, styrene-methyl methacrylate-graft polymers, (styrene-glycidyl methacrylate)-methyl methacrylate-graft copolymers, acid-modified acrylic-styrene-graft polymers, (styrene-glycidyl methacrylate)-styrene-graft polymers, polybutylene terephthalate-polystyrene-graft polymers, polyphenylene ether, (styrene-maleic anhydride)-polyphenylene ether-graft polymers, maleic anhydride-modified polyphenylene ether, fumaric acid-modified polyphenylene ether, glycidyl methacrylate-modified polyphenylene ether, amine-modified polyphenylene ether and other modified polyphenylene ether polymers. Among them, unmodified or modified polyphenylene ether is preferred, and maleic anhydride-modified polyphenylene ether and fumaric acid-modified polyphenylene ether are more preferred.

[0038] Although the modified polyphenylene ether can be obtained by modifying a known polyphenylene ether using a modifier, the modified polyphenylene ether is not limited to this method as long as it can be used for the purpose of the present invention. The polyphenylene ether is a known compound. Based on its purpose, reference can be made to the specifications of U.S. Patents No. 3,306,874, No. 3,306,875, No. 3,257,357 and No. 3,257,358. Polyphenylene ether can usually be prepared by an oxidative coupling reaction using a disubstituted or trisubstituted phenol in the presence of a copper amine complex catalyst. The copper amine complex can use a copper amine complex derived from a primary amine, a secondary amine and a tertiary amine.

[0039] Examples of the polyphenylene ether include poly(2,3-dimethyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-chloromethyl-1,4-phenylene ether), poly(2-methyl-6-hydroxyethyl-1,4-phenylene ether), poly(2-methyl-6-n-butyl-1,4-phenylene ether), poly(2-ethyl-6-isopropyl-1,4-phenylene ether), poly(2-ethyl-6-n-propyl-1,4-phenylene ether), poly(2,3,6-trimethyl-1,4-phenylene ether), poly[2-(4'-methylphenyl)-1,4-phenylene ether], poly(2-bromo-6-phenyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2-phenyl 4-phenylene ether), poly(2-chloro-1,4-phenylene ether), poly(2-methyl-1,4-phenylene ether), poly(2-chloro-6-ethyl-1,4-phenylene ether), poly(2-chloro-6-bromo-1,4-phenylene ether), poly(2,6-di-n-propyl-1,4-phenylene ether), poly(2-methyl-6-isopropyl-1,4-phenylene ether), poly(2-chloro-6-methyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dibromo-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether) and poly(2,6-dimethyl-1,4-phenylene ether), etc.

[0040] For example, copolymers derived from two or more phenolic compounds used to prepare the above-mentioned polyphenylene ethers can also be used. Furthermore, graft copolymers and block copolymers of vinyl aromatic compounds such as polystyrene and the above-mentioned polyphenylene ethers can also be cited. In particular, poly(2,6-dimethyl-1,4-phenylene ether) is preferably used.

[0041] As the modifier for modifying the polyphenylene ether, compounds having ethylenic double bonds and polar groups in the same molecule can be cited, and specifically, for example, maleic anhydride, maleic acid, fumaric acid, maleic esters, fumaric esters, maleimide and N-substituted products thereof, maleates, fumarates, acrylic acid, acrylates, acrylamides, acrylates, methacrylic acid, methacrylates, methacrylic acid amides, methacrylates, glycidyl methacrylate, etc. can be cited. Among these, maleic anhydride, fumaric acid and glycidyl methacrylate are particularly preferably used. The above-mentioned various modifiers can be used alone or in combination of two or more.

[0042] For example, the modified polyphenylene ether can be obtained by reacting the above-mentioned polyphenylene ether with a modifier in the presence of a solvent or other resin. The modification method is not particularly limited, and a known method can be used. Specifically, there can be cited a method of melt-kneading and reacting it at a temperature in the range of 150 to 350°C using a roll mill, a Banbury mixer, an extruder, etc.; a method of heating and reacting it in a solvent such as benzene, toluene, and xylene, etc. Furthermore, in order to facilitate the reaction, it is also an effective method to allow a free radical initiator such as benzoyl peroxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, tert-butyl perbenzoate, azobisisobutyronitrile, azobisisovaleronitrile, 2,3-diphenyl-2,3-dimethylbutane to be present in the reaction system. A method of melt-kneading in the presence of a free radical initiator is particularly preferred.

[0043] The polar group content in the polyphenylene ether is expected to be in the range of 0.01 to 20% by mass, preferably 0.05 to 10% by mass. When the content is less than 0.01% by mass, the effect as a compatibilizer cannot be fully exerted, and when it exceeds 20% by mass, the compatibility with the styrene polymer (A) having a syndiotactic structure decreases. The mixing amount of the polyphenylene ether is 0.1 to 10% by mass relative to the total weight of the resin component, preferably 0.5 to 8% by mass. When it is less than 0.1% by mass, the effect as a compatibilizer is insufficient. When it exceeds 20% by mass, the heat resistance of the composition decreases significantly.

[0044] [Non-fibrous filler (D)] The non-fibrous filler (D) (hereinafter also referred to as component (D)) is a non-fibrous filler that can be expected to suppress the linear expansion coefficient and dimensional change in the parallel direction (MD) and the perpendicular direction (TD) relative to the extrusion direction of the sheet forming body. As the non-fibrous filler (D), known shapes such as spherical, granular, and plate-like can be used. Any of inorganic and organic fillers are acceptable, preferably spherical, granular or plate-like fillers of inorganic systems, for example, talc, carbon black, graphite, titanium dioxide, silicon dioxide, mica, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, oxysulfate, tin oxide, aluminum oxide, kaolin, silicon carbide, metal powder, glass powder, glass flakes, glass beads, etc.

[0045] From the viewpoint of productivity, cost and dielectric properties of the filler itself, among these inorganic fillers, silica is particularly preferred, and amorphous silica or fused silica is more preferred. Amorphous silica has a lower hardness than crystalline silica, and can suppress wear of machinery and screws.

[0046] Fused silica is produced by melting raw materials in flames and rapidly cooling the volatilized gas to solidify. Due to its surface tension, it becomes spherical and has fewer sharp parts. The filler itself does not disintegrate and can be easily formed into a stable shape.

[0047] The shape of silica is preferably granular or spherical silica, and more preferably spherical silica. By making the shape of silica granular or spherical, when adding silica to molten resin, it is easy to mix. In addition, since it is also stable to apply force from any direction, the decline of the mechanical properties of the sheet forming body is less, and silica is difficult to be destroyed and separated from the sheet forming body.

[0048] The D50 average particle size of the non-fibrous filler (D) is preferably 0.1 to 45 μm. It is more preferably 0.2 to 30 μm, and further preferably 0.3 to 20 μm. By making the D50 average particle size 0.1 μm or more, the aggregation of the (D) components can be suppressed, and they will not become foreign matter in the sheet forming body, and the mechanical properties will not decrease. In addition, by making the D50 average particle size 45 μm or less, the intervals between the (D) components will not be too narrow, and the propagation of cracks at the interface when stress is generated can be suppressed. In addition, the heat resistance under the welding process can be maintained.

[0049] The content of the non-fibrous filler (D) is preferably 1 to 60 parts by mass relative to 100 parts by mass of the polystyrene polymer (A) having a syndiotactic structure. It is more preferably 3 to 50 parts by mass, and further preferably 5 to 40 parts by mass. When the content is 1 part by mass or more, the effect of the component (D) can be shown. In addition, by making the content less than 60 parts by mass, in addition to the good smoothness of the surface of the sheet forming body and the ease of film thickness control, it is also possible to suppress the aggregation of the components (D) in the sheet forming body and suppress the decline in mechanical properties.

[0050] In the case of hollow objects of amorphous silica and fused silica, the above content is not followed. By using hollow silica, the dielectric constant can be expected to be further reduced. When using hollow silica, the film thickness is preferably in the range of 0.5 to 2.0 μm, more preferably 0.5 to 1.5 μm, and further preferably in the range of 0.5 to 1.2 μm. When the film thickness becomes too thin, the silica breaks during screw mixing in a twin-shaft mixer, and there is a situation where the hollow shape cannot be maintained. When the film thickness becomes too thick, due to the reduction in the volume fraction of the hollow part, there is a situation where the effect of reducing the dielectric constant cannot be exerted. The D50 average particle size of the hollow silica is preferably in the range of 3 to 45 μm. When the particle size is less than 3 μm, the effect of reducing the dielectric constant cannot be expected, and when the particle size exceeds 45 μm, there is a situation where the mechanical properties of the sheet forming body decrease.

[0051] The non-fibrous filler (D) may be either surface treated or untreated. The surface treatment agent may be any known surface treatment agent, but by using a silane / titanate coupling agent to perform a hydrophobic treatment, the dispersion state in the styrene polymer (A) having a syndiotactic structure is improved, the mechanical properties of the sheet are improved, and the generation of agglomerates can be suppressed.

[0052] As the organic spherical, granular or plate-shaped filler, there is no particular limitation on the polymer used, but in consideration of the processing temperature of the styrene resin (A) having a syndiotactic structure, the melting point is preferably higher than 280° C., and more preferably higher than 300° C. for a crystalline resin. In addition, in the case of an amorphous resin, the glass transition temperature is preferably higher than 150° C., and more preferably higher than 180° C. By setting the melting point and the glass transition temperature within the above range, the shape of the filler can be maintained during the processing of the sheet molded body, and the linear expansion coefficient of the sheet molded body can be suppressed.

[0053] <Antioxidant (E)> From the viewpoint of processability, the sheet forming body of the present invention may also contain the following antioxidant (E) (hereinafter also referred to as component (E)). As the antioxidant (E) in the present invention, it can be any one of a primary antioxidant that captures the generated free radicals and prevents oxidation or a secondary antioxidant that decomposes the generated peroxide to prevent oxidation. As the primary antioxidant, phenolic antioxidants and amine antioxidants can be mentioned; as the secondary antioxidant, phosphorus antioxidants and sulfur antioxidants can be mentioned. By using these antioxidants alone or in combination, the molecular weight decrease of component (A) or (B) when manufacturing the SPS resin composition can be suppressed, and the generation of gas from component (A) or (B) can be suppressed in the hot pressing process when manufacturing the sheet forming body.

[0054] Specific examples of phenolic antioxidants include monophenolic antioxidants such as 2,6-di-tert-butyl-4-methylphenol, 2,6-di-tert-butyl-4-ethylphenol, 2-tert-butyl-4-methoxyphenol, 3-tert-butyl-4-methoxyphenol, 2,6-di-tert-butyl-4-[4,6-bis(octylthio)-1,3,5-triazin-2-ylamino]phenol, and n-octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate. In addition, bisphenol antioxidants such as 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylenebis(3-methyl-6-tert-butylphenol), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], and 3,9-bis[1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane can be mentioned. In addition, high molecular weight phenolic antioxidants such as 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[3,3'-bis-(4'-hydroxy-3'-tert-butylphenyl)butyric acid]diol ester, 1,3,5-tris(3',5'-di-tert-butyl-4'-hydroxybenzyl)-secondary triazine-2,4,6-(1H,3H,5H)trione, and d-α-tocopherol can be mentioned.

[0055] Specific examples of the amine antioxidant include alkyl-substituted diphenylamine and the like.

[0056] Specific examples of phosphorus-based antioxidants include triphenyl phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, 4,4'-butylene-bis(3-methyl-6-tert-butylphenyl di(tridecyl))phosphite, octadecyl phosphite, tri(nonylphenyl)phosphite, diisodecyl pentaerythritol diphosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(3,5-di-tert-butyl-4 -hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)octylphosphite, etc.

[0057] Specific examples of the sulfur-based antioxidant include dilauryl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, dioctadecyl 3,3'-thiodipropionate, pentaerythritol tetrakis(3-laurylthiopropionate), and 2-mercaptobenzimidazole.

[0058] From the viewpoint of being able to suppress the heat resistance of the sheet, thermal degradation during processing, etc., the antioxidant is preferably a primary antioxidant, and a phenolic antioxidant is particularly preferred. The antioxidant preferably has a thermal decomposition temperature of 250°C or more. When the thermal decomposition temperature is high, the effect of improving the insulation breakdown voltage at high temperature is improved. When the thermal decomposition temperature is too low, the antioxidant itself undergoes thermal decomposition during melt extrusion, which tends to easily cause problems such as process contamination and polymer coloring yellow, and is therefore not preferred. From this viewpoint, the thermal decomposition temperature of the antioxidant is more preferably above 280°C, further preferably above 300°C, and particularly preferably above 320°C. The antioxidant in the present invention is preferably an antioxidant that is difficult to thermally decompose, and although the higher the thermal decomposition temperature, the more preferred, the upper limit is actually below 500°C.

[0059] In addition, the melting point of the antioxidant is preferably above 90°C. When the melting point is too low, the antioxidant melts earlier than the polymer during melt extrusion, and there is a tendency for the polymer to slip in the screw supply part of the extruder. Therefore, the supply of the polymer becomes unstable, resulting in problems such as uneven thickness and deterioration of the sheet. From this point of view, the melting point of the antioxidant is more preferably above 120°C, further preferably above 150°C, and particularly preferably above 200°C. On the other hand, when the melting point of the antioxidant is too high, the antioxidant tends to be difficult to melt during melt extrusion, and the dispersion in the polymer deteriorates. Therefore, problems such as the effect of adding the antioxidant can only be manifested locally are generated. From this point of view, the melting point of the antioxidant is preferably below 300°C, more preferably below 250°C, further preferably below 220°C, and particularly preferably below 170°C.

[0060] As the antioxidants described above, commercially available products may be used as they are. Examples of commercially available products include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (manufactured by Ciba Specialty Chemicals: trade name IRGANOX1010), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine (manufactured by Ciba Specialty Chemicals: trade name IRGANOX1024), and N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] (manufactured by Ciba Specialty Chemicals: trade name IRGANOX1098).

[0061] Based on the mass of the polystyrene resin composition, the content of the antioxidant is preferably 0.1% by mass or more and 8% by mass or less. By containing an antioxidant in the above-mentioned numerical range, the heat resistance / heat degradation resistance of the sheet can be improved. When the content of the antioxidant is too little, the effect of adding the antioxidant tends to be insufficient, and the effect of improving the dielectric breakdown voltage is reduced. From this point of view, the content of the antioxidant is more preferably 0.2% by mass or more, further preferably 0.3% by mass or more, and particularly preferably 0.5% by mass or more. On the other hand, when the content is too much, the antioxidant in the sheet tends to be easy to condense, and the shortcomings from the antioxidant increase, and the mechanical properties of the sheet are reduced due to the relevant shortcomings. From this point of view, the content of the antioxidant is more preferably 6% by mass or less, further preferably 4% by mass or less, and particularly preferably 2% by mass or less.

[0062] The antioxidant may be used alone or in combination of two or more. When two or more are used in combination, it may be a method of using two or more primary antioxidants, a method of using two or more secondary antioxidants, or a method of using one or more primary antioxidants and one or more secondary antioxidants in combination. For example, by using two antioxidants, a primary antioxidant and a secondary antioxidant in combination, it is expected to prevent both primary oxidation and secondary oxidation. In the present invention, from the viewpoint of being able to further improve the effect of suppressing thermal degradation during processing, it is preferred to use a primary antioxidant alone or use two or more primary antioxidants, and it is particularly preferred to use a phenolic antioxidant alone or use two or more phenolic antioxidants.

[0063] The sheet formed article of the present invention may also contain flame retardants / release agents / lubricants / viscosity reducing agents / curing agents other than those mentioned above. The flame retardant is not particularly limited, but halogen-based, organic or inorganic phosphates / phosphate esters / phosphorus copolymers containing bromine may be used appropriately. The flame retardant used may be liquid or solid, but from the viewpoint of long-term stability, it is preferred to use a flame retardant that is solid at room temperature.

[0064] <Polystyrene Resin Composition> The polystyrene resin composition is a composition containing at least the predetermined components (A), (C) and (D), and further containing components (B) and (E) as required. The sheet forming body of the present invention can be manufactured using the polystyrene resin composition. The polystyrene resin composition is preferably prepared by mixing the components in predetermined amounts, kneading, and pelletizing.

[0065] <Sheet Formed Body> The sheet forming body of the present invention is a non-stretched sheet forming body. The so-called non-stretching does not only mean no stretching at all, but also some residual strain may exist. Specifically, in the parallel direction (longitudinal direction, MD) and the perpendicular direction (transverse direction, TD) relative to the extrusion direction of the sheet forming body, the stretching ratio is preferably 1.3 or less, more preferably 1.2 or less, further preferably 1.1 or less, and most preferably 1.0. By making the stretching ratio within the above range, the dimensional change rate (low thermal shrinkage) of the sheet forming body can be reduced.

[0066] Regarding the sheet formed body of the present invention, at a temperature of 23° C., a relative humidity of 50%, and a frequency of 10 GHz, the relative dielectric constant is 3 or less. It is preferably 2.8 or less, and more preferably 2.7 or less. When the relative dielectric constant is 3 or less, the signal transmission speed is fast and the dielectric loss can be reduced. The lower limit is not particularly limited, but it can be 1.0 or more in industry, and it does not matter if it is 2.0 or more.

[0067] The dielectric loss tangent of the sheet formed body of the present invention at a temperature of 23°C, a relative humidity of 50%, and a frequency of 10 GHz is preferably 0.002 or less. It is more preferably 0.0015 or less, and further preferably 0.001 or less. When the dielectric loss tangent is 0.002 or less, the dielectric loss can be suppressed, and the performance as a circuit substrate in high frequency is good. The lower limit is not particularly limited, and it can be 0.0001 or more, and it does not matter if it is 0.0002 or more.

[0068] The linear expansion coefficients of the sheet formed product of the present invention in the longitudinal direction (MD) and the transverse direction (TD) are each preferably 10 to 80 ppm / °C, more preferably 15 to 75 ppm / °C, and further preferably 20 to 70 ppm / °C. In addition, the MD / TD ratio is preferably 0.6 to 1.4, more preferably 0.65 to 1.35, and further preferably 0.7 to 1.3.

[0069] The dimensional change rates of the sheet formed article of the present invention in the machine direction (MD) and the transverse direction (TD) after heat treatment at 150°C for 30 minutes are each preferably less than 0.4%, more preferably 0.3% or less, and even more preferably 0.2% or less.

[0070] The film thickness of the sheet formed body of the present invention is preferably 10 μm to 2000 μm, more preferably 20 μm to 1000 μm, further preferably 30 μm to 500 μm, and most preferably 50 μm to 350 μm. When the film thickness is less than 10 μm, the sheet formed body is easily broken; when it is greater than 2000 μm, there is a possibility that the sheet will be drawn down due to its own weight when extruded, or partial shrinkage will occur, resulting in uneven film thickness of the sheet. Example

[0071] The present invention will be described in further detail with reference to the following examples, but the present invention is not limited to these examples. In the following examples, parts and % are expressed on a mass basis unless otherwise specified.

[0072] (1) Raw materials used in Examples and Comparative Examples <Styrene polymer having a syndiotactic structure (A)> A1: XAREC (registered trademark) 130ZC (manufactured by Idemitsu Kosan Co., Ltd., syndiotactic polystyrene 100% by mass, MFR = 15 g / 10 min, measurement temperature: 300°C, load: 1.2 kg, not modified with a compound having a polar group) A2: XAREC (registered trademark) 90ZC (manufactured by Idemitsu Kosan Co., Ltd., syndiotactic polystyrene 100% by mass, MFR = 9 g / 10 min, measurement temperature: 300°C, load: 1.2 kg, not modified with a compound having a polar group)

[0073] <Rubber-like elastic body (B)> B1: Toughtech (registered trademark) H1062 (manufactured by Asahi Kasei Corporation, styrene ratio = 18% by mass, MFR = 4.5 g / 10 minutes, measurement temperature: 230° C., load: 2.16 kg) B2: Toughtech (registered trademark) H1041 (manufactured by Asahi Kasei Corporation, styrene ratio = 30% by mass, MFR = 5.0 g / 10 minutes, measurement temperature: 230°C, load: 2.16 kg) B3: Toughtech (registered trademark) H1517 (manufactured by Asahi Kasei Corporation, styrene ratio = 43% by mass, MFR = 3.0 g / 10 minutes, measurement temperature: 230° C., load: 2.16 kg) B4: Toughtech (registered trademark) H1521 (manufactured by Asahi Kasei Corporation, styrene ratio = 18% by mass, MFR = 15.0 g / 10 minutes, measurement temperature: 230°C, load: 2.16 kg)

[0074] <Fibrous filler (C)> C1: HDT09100T (manufactured by TOCHU, fiber diameter: 9 μm, D50 average fiber length: 100 μm, D glass) C2: EPH80M-01N (manufactured by Nippon Electric Glass Co., Ltd., fiber diameter: 10 μm, D50 average fiber length: 80 μm, E glass) C3: EFH30-01 (manufactured by Central Fiberglass, fiber diameter: 11 μm, D50 average fiber length: 30 μm, E glass) C4: ECS301HP-3-H (manufactured by Chongqing International Composite Materials Co., Ltd., fiber diameter: 10μm, D50 average fiber length: 3000μm, E glass) C5: ChopVantage HP-3610 (manufactured by Nippon Electric Glass Co., Ltd., fiber diameter: 10 μm, D50 average fiber length: 4500 μm, E glass)

[0075] <Non-fibrous filler (D)> D1: Silica particles: FB-3SDC (manufactured by Denka, D50 average particle size: 3.1 μm) D2: Silica particles: FB-7SDC (manufactured by Denka, D50 average particle size: 5.4 μm) D3: Silica particles: SFP-130MC (manufactured by Denka, D50 average particle size: 0.6 μm) D4: Hollow glass microspheres: iM-30k (manufactured by 3M Japan, D50 average particle size: 17μm) D5: Calcium carbonate: Whiten P-30 (Whitestone Calcium Industry Co., Ltd., D50 average particle size: 4.8 μm) D6: Magnesium oxide: RF-98 (manufactured by Ube Materials, D50 average particle size: 50 μm)

[0076] <Antioxidant (E)> E1: ANOX20 (manufactured by BASF Japan, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], E2: PEP-36 (manufactured by ADEKA, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane)

[0077] <Method for producing polystyrene resin composition> In order to obtain the sheet formed article of the present invention, a polystyrene resin composition (SPS resin composition) is produced by mixing and kneading the above-mentioned various components including SPS and the respective components (A) to (D) and (E) to obtain a composition.

[0078] More specifically, use The same-direction twin-screw extruder (resin temperature: 300°C) feeds (A) to (D) and (E) from the main feeder or side feeder, mixes them, and discharges them from the circular die. After forming strands, the strands were cooled and solidified using a water cooling bath, and cylindrical pellets of the SPS resin composition were obtained by cutting.

[0079] <Method for producing sheet molded article> The pellets of the SPS resin composition obtained by the above-mentioned production method are put into The resin was remelted in the hopper of a single-axis screw extruder (resin temperature: 300°C), extruded into a sheet by a T-die, and clamped by two rollers (temperature: 90°C). After compression and cooling and solidification, it was wound on a paper tube with a diameter of 80mm at a speed of 1m / min to obtain an unstretched SPS sheet with a thickness of 300μm. At this time, as an evaluation of the winding property of the roller, no adhesion to the cooling roller was observed, and no uneven thickness on the surface of the sheet was observed (○), adhesion to the roller or uneven thickness on the surface of the sheet was observed (△), although there was no adhesion to the roller, uneven thickness or tiny cracks on the surface of the sheet were observed (△△), and it was impossible to wind due to adhesion to the roller and rupture of the surface of the sheet (×). Below, relative to the extrusion direction of the sheet, the parallel direction is defined as MD, and the perpendicular direction is defined as TD.

[0080] <Heat treatment and humidity control process> By subjecting the obtained unstretched SPS sheet to heat treatment, the crystallinity of the component (A) contained in the SPS sheet is increased, and the soldering heat resistance of the SPS sheet can be improved. The SPS sheet obtained by the above-mentioned manufacturing method was clamped with a commercially available polyimide film (manufactured by Ube Industries, Ltd., Upilex) and a silicon sheet, and compressed and heated using a hydraulic manual press (under vacuum, temperature: 200°C, time: 30 min, pressure: 2 MPa). The obtained heat-treated SPS sheet (hereinafter referred to as the sheet molding) was subjected to a 24-hour humidity conditioning treatment in an environment of 23°C×50%RH to eliminate the influence of humidity and obtain a sample with less deviation caused by external factors. At this time, the appearance of the sheet molding was observed, and obvious bubbling was observed on the surface (△△), no bubbling was observed but partial transfer unevenness was observed due to gas generated by resin decomposition during hot pressing (△), and a clean glossy surface or a uniform matte surface was obtained (○).

[0081] In order to confirm whether the crystallization of the sheet forming body is complete, a differential scanning calorimeter (manufactured by Hitachi High-tech Science Co., Ltd., DSC7020) was used to perform an evaluation based on JIS K7121 (2012). More specifically, 5 mg of the sheet forming body was placed in an aluminum pan, and when the temperature was raised from room temperature at a rate of 20° C. / min, it was confirmed that no exothermic peak was observed in the temperature range of 100 to 220° C., thereby confirming that crystallization was completed by the heat treatment during pressing. In the following paragraphs, the sheet formed body subjected to the heat treatment and the humidity control treatment was evaluated for properties 1 to 4.

[0082] In the case of preparing a biaxially stretched sheet formed body, a non-stretched SPS sheet having a thickness of 500 μm was prepared by the same method as above, and then biaxially stretched (temperature: 110° C., stretching ratio: 3.3×3.4 (MD×TD), stretching speed: 500% / min). Thereafter, a relaxation heat treatment was performed in a hot drying furnace (temperature: 230° C., relaxation ratio: 0.95×0.95 (MD×TD)) to obtain a biaxially stretched SPS sheet having a film thickness of 50 μm.

[0083] <Evaluation method> 1. Dielectric properties The sheet forming body is sliced ​​to make a short strip test piece of MD direction: 3mm × TD direction: 80mm. Then, under the test environment of temperature: 23°C / humidity: 50%, the dielectric properties (relative dielectric constant: Dk / dielectric loss tangent: Df) of the test piece at a frequency of 10GHz are measured for a total of 5 times, and the average value is calculated (based on JIS C2565). As a measuring device, an MS46122B network analyzer manufactured by Anritsu and a cavity resonator manufactured by AET Co., Ltd. are used. The relative dielectric constant (Dk) is qualified (○) below 3, and unqualified (×) for more than 3. In addition, the dielectric loss tangent (Df) is qualified (○) below 0.002, and unqualified (×) for more than 0.002.

[0084] 2. Linear expansion coefficient (TMA) The sheet forming body is sliced, and short strip test pieces with a width direction of 3mm×vertical direction of 25mm are made in the MD direction (test piece with the length direction in the MD direction) and the TD direction (test piece with the length direction in the TD direction). Then, the linear expansion coefficient of each test piece in the obtained MD direction and TD direction is measured 5 times each, and the average value is calculated (based on JIS K7197). As a measuring device, TMA7100 manufactured by Hitachi High-tech Science Co., Ltd. is used, and the measurement is carried out under the condition of a load of 2gf / mm. The reading range of the measurement results is carried out in the temperature range of 23℃ to 80℃, and the linear expansion coefficients in the MD direction and the TD direction are both above 10ppm / ℃ and below 80ppm / ℃ to be qualified.

[0085] 3. Dimensional change rate The sheet was sliced ​​to make a rectangular test piece with a length of 180 mm in the MD direction and 130 mm in the TD direction. Straight lines were drawn on the surface of the test piece in parallel to the MD direction and the TD direction, and intersected at the midpoint to form a quadrilateral with a length of 120 mm × 70 mm (MD × TD). The length of the straight lines in the MD / TD direction of the test piece was measured respectively. Next, in a hot air circulation furnace set at an atmosphere of 150°C, place it in a suspended state with one corner supported for 30 minutes, then take the test piece out of the furnace and cool it in an environment of temperature: 23°C / humidity: 50% RH for 24 hours to remove the influence of moisture content. After that, measure the straight line length in the MD / TD direction respectively, and find the change from the length measured before the test of 150°C / 30 minutes, and find the ratio of the change in each length relative to the test as the thermal shrinkage rate. When the thermal shrinkage rate value is positive, it indicates shrinkage. It should be noted that when the absolute value of the thermal shrinkage rate is less than 0.4%, it is qualified (○), and when it is more than 0.4%, it is unqualified (×).

[0086] 4. Welding heat resistance test The sheet molded body was sliced ​​to make a test piece of 50 mm in MD direction × 50 mm in TD direction. Then, the test sheet was floated in a solder bath heated to 260°C for 120 seconds, and the degree of deformation and the presence of abnormal appearance such as blistering were visually observed. The case where no deformation or blistering of the appearance was observed was rated as (◎), the case where no significant deformation or blistering of the appearance was observed was rated as qualified (○), the case where some wrinkles were observed was rated as barely qualified (△), and the case where significant deformation or blistering of the appearance was observed was rated as unqualified (×).

[0087] (Examples 1 to 23) Examples 1 to 12 containing predetermined amounts of the above-mentioned components (A), (C) and (D) can satisfy the required physical properties and exhibit overall well-balanced performance. The results are shown in Tables 1 and 2.

[0088] (Comparative Examples 1 to 8) When the above-mentioned components (A), (C) and (D) were added in excessive or insufficient amounts, some physical properties could not be satisfied as in Comparative Examples 1 to 12, and the quality of the sheet products was poor.

[0089] [Table 1]

[0090] [Table 2]

[0091] [Table 3] Industrial Applicability

[0092] As is clear from the above description, according to the present invention, the dielectric properties, linear expansion coefficient, dimensional stability and soldering heat resistance of the sheet molded body described in the embodiment all show excellent properties, and it is expected that the sheet molded body of the present invention will be used in electronic components, antenna components, etc. for communication equipment requiring 5G.

Claims

1. A sheet-like formed article comprising a styrene polymer (A) having a syndiotactic structure, a fibrous filler (C) and a non-fibrous filler (D), The sheet material formed body is a non-stretched sheet material formed body, The fibrous filler (C) is contained in an amount of 1 to 50 parts by mass relative to 100 parts by mass of the styrene polymer (A) having a syndiotactic structure, The sheet formed body has a relative dielectric constant of 3 or less in a frequency band of 10 GHz. 2 . The sheet formed article according to claim 1 , comprising 1 to 40 parts by mass of a rubber-like elastic body (B) based on 100 parts by mass of the styrene polymer (A) having a syndiotactic structure. 3 . The sheet formed article according to claim 1 , wherein the fibrous filler (C) is glass fiber having a D50 average fiber length of 40 to 4000 μm. 4 . The sheet-shaped article according to claim 1 , wherein the non-fibrous filler (D) is a granular or spherical filler having a D50 average particle size of 0.1 to 45 μm. 5 . The sheet formed article according to claim 1 , wherein the rubber-like elastic body (B) contains a styrene-based or olefin-based thermoplastic elastomer. 6 . The sheet formed article according to claim 1 , wherein the linear expansion coefficients of the sheet formed article in the longitudinal direction MD and the transverse direction TD are 10 to 80 ppm / ° C., and the ratio MD / TD is within the range of 0.6 to 1.

4. 7 . The sheet formed article according to claim 1 , wherein the absolute value of the dimensional change rate of the sheet formed article after heat treatment at 150° C. for 30 minutes is less than 0.4%.

Citation Information

Patent Citations

  • Printed wiring board laminate material

    JP1995142830A

  • Copolymers of polyphenylene ethers

    US3257357A

  • 2, 6-dichloro-1, 4-polyphenylene ether

    US3257358A

  • Oxidation of phenols

    US3306874A

  • Oxidation of phenols and resulting products

    US3306875A