Adhesive structure and method for manufacturing same, electronic device and method for manufacturing same, and adhesive layer for transfer
By using patterned adhesive parts and low elastic parts on the electronic circuit substrate and combining the thermal conductivity parts, the problems of insufficient heat resistance and stress relief performance are solved, and high-integration and high-speed chip bonding and connection are achieved , improves the overall performance of electronic components.
Patent Information
- Application Number
- CN202380027607.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-29
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-08
AI Technical Summary
When it is difficult to achieve highly integrated and high-speed chip bonding and connection in electronic circuit substrates, the heat resistance reliability and stress relief performance are insufficient, mainly due to the thermal stress problems caused by the difference in linear thermal expansion coefficients between semiconductors and substrates.
Using an adhesive portion with a patterned shape and a low elastic portion, a patterned adhesive structure is formed by inkjet method, and combined with a thermal conduction portion, the deformation characteristics of the adhesive layer thickness and plane direction are optimized, and the adhesion and stress are improved. Relieve performance.
The thin film structure with excellent adhesion, heat resistance and stress relief characteristics is achieved, which enhances the heat resistance reliability and production efficiency of electronic components, reduces the generation of bubbles and voids, and improves the thermal conductivity.
Smart Images

Figure BDA0005042438130000121 
Figure BDA0005042438130000131 
Figure BDA0005042438130000151
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive structure and a method for producing the same, an electronic component and a method for producing the same, and an adhesive layer for transfer. Background Art
[0002] In electronic circuit substrates, along with high integration and high speed, the temperature rise caused by heating elements such as IC chips increases, and there is a requirement for heat-resistant reliability of bonding and connection of installed circuits. As the main reason for the reduction of bonding and connection reliability, thermal stress caused by the difference in linear thermal expansion coefficients between the semiconductor (chip) and the various materials bonded to the semiconductor (chip) can be cited. Specifically, the linear thermal expansion coefficient of the semiconductor (chip) is about 3ppm / K, while the linear thermal expansion coefficient of the mounting substrate is as large as more than 15ppm / K. Therefore, thermal stress is generated due to thermal cycles caused by heating production process steps such as reflow and drive heating, which makes it easy for poor bonding and connection of the semiconductor (chip) to occur.
[0003] In the past, as chip bonding components for bonding chips to chips and chips to substrates, solution-based chip bonding pastes and sheet-like chip bonding films were used. In the chip bonding film, it is proposed to use epoxy resin, curing agent, and polymer compounds that are incompatible with epoxy resin to form a phase-separated island structure of a bonding portion composed of epoxy resin and a polymer compound having stress relaxation properties during curing, thereby improving heat resistance reliability (see patent document 1). In addition, an adhesive layer (APROXTM (registered trademark) BP, manufactured by Nippon Shokubai Co., Ltd.) in which rubber (low elasticity portion) is mixed in the epoxy resin (adhesive portion) has also been proposed. In addition, it is also known that a chip bonding element that is endowed with thermal conductivity as a heat dissipation function in addition to the bonding function is also known.
[0004] Citation list
[0005] Patent Literature
[0006] [Patent Literature]
[0007] [Patent Document 1] Japanese Unexamined Patent Application Publication No. 2011-084743 Summary of the invention
[0008] Technical issues
[0009] An object of the present invention is to provide an adhesive structure which is excellent in adhesiveness, heat resistance and stress relaxation properties and can be reduced in thickness.
[0010] Solutions to the problem
[0011] The adhesive structure of the present embodiment as a solution to the above problem includes: an adhesive portion that adheres to a contact object, and a low elastic portion having an elastic modulus lower than that of the adhesive portion, wherein at least one of the adhesive portion and the low elastic portion has a pattern shape.
[0012] Effects of the Invention
[0013] According to the present invention, it is possible to provide an adhesive structure which is excellent in adhesiveness, heat resistance and stress relaxation properties and can be reduced in thickness. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] A more complete understanding of the embodiments and many of the attendant advantages and features thereof can be readily obtained and understood from the following detailed description taken in conjunction with the accompanying drawings.
[0015] [ Figure 1A ]
[0016] Figure 1A is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0017] [ Figure 1B ]
[0018] Figure 1B yes Figure 1A Schematic cross-sectional view of the adhesive structure in the plane direction.
[0019] [ Figure 2A ]
[0020] Figure 2A This is a schematic cross-sectional view of a conventional adhesive layer having stress relaxation properties in the thickness direction.
[0021] [ Figure 2B ]
[0022] Figure 2B yes Figure 2A A schematic cross-sectional view of a conventional adhesive layer having stress relaxation properties in a plane direction.
[0023] [ Figure 3A ]
[0024] Figure 3A is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0025] [ Figure 3B ]
[0026] Figure 3B is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0027] [ Figure 3C ]
[0028] Figure 3C is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0029] [ Figure 3D ]
[0030] Figure 3D is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0031] [ Figure 3E ]
[0032] Figure 3E is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0033] [ Figure 3F ]
[0034] Figure 3F is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0035] [ Figure 3G ]
[0036] Figure 3G is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0037] [ Figure 3H ]
[0038] Figure 3H is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0039] [ Fig. 3I ]
[0040] Fig. 3I is a schematic cross-sectional view of an adhesive structure according to an embodiment of the present invention in the thickness direction.
[0041] [ Figure 4A ]
[0042] Figure 4A is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0043] [ Figure 4B ]
[0044] Figure 4B is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0045] [ Figure 4C ]
[0046] Figure 4C is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0047] [ Figure 4D ]
[0048] Figure 4D is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0049] [ Figure 4E ]
[0050] Figure 4E is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0051] [ Figure 4F ]
[0052] Figure 4F is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0053] [ Figure 4G ]
[0054] Figure 4G is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0055] [ Figure 4H ]
[0056] Figure 4H is a schematic top view in a planar direction of an adhesive structure according to an embodiment of the present invention.
[0057] [ Figure 5 ]
[0058] Figure 5 is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0059] [ Figure 6 ]
[0060] Figure 6 is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0061] [ Fig. 7A ]
[0062] Fig. 7A is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0063] [ Figure 7B ]
[0064] Figure 7B is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0065] [ Fig. 8A ]
[0066] Fig. 8A is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0067] [ Figure 8B ]
[0068] Figure 8B is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0069] [ Fig. 9A ]
[0070] Fig. 9A is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0071] [ Fig. 9B ]
[0072] Fig. 9B is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0073] [ Fig.10 ]
[0074] Fig.10 is a schematic cross-sectional view of an electronic component using an adhesive structure according to an embodiment of the present invention.
[0075] [ Fig.11A ]
[0076] Fig.11A is a schematic cross-sectional view of a configuration in which the adhesive structure of Example 1 is used.
[0077] [ Fig. 11B ]
[0078] Fig. 11B is a schematic top view of a configuration in which the adhesive structure of Example 1 is used.
[0079] [ Fig. 12A ]
[0080] Fig. 12A is a schematic cross-sectional view of a configuration in which the adhesive structure of Example 5 is used.
[0081] [ Fig. 12B]
[0082] Fig. 12B is a schematic top view of a configuration in which the adhesive structure of Example 5 is used.
[0083] [ Fig.13 ]
[0084] Fig.13 This is a scanning electron microscope (SEM) photograph of the heat transfer portion of Test Example 1.
[0085] The accompanying drawings are intended to describe embodiments of the present disclosure and should not be interpreted as limiting the scope thereof. Unless explicitly noted, the accompanying drawings should not be considered to be drawn to scale. Moreover, throughout the several views, the same or similar reference numerals represent the same or similar components. DETAILED DESCRIPTION
[0086] In describing the embodiments shown in the drawings, specific terms are used for clarity. However, the disclosure of this specification is not intended to be limited to the specific terms selected, and it should be understood that each specific component includes all technical equivalents having similar functions, operating in a similar manner and achieving similar results.
[0087] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0088] (Adhesive structure and method for producing the adhesive structure)
[0089] The adhesive structure of the present invention comprises: an adhesive portion to be bonded to a contact object, and a low elastic portion having an elastic modulus lower than that of the adhesive portion, wherein at least one of the adhesive portion and the low elastic portion has a pattern shape, and may optionally include a heat conducting portion, and may also optionally include other components.
[0090] The pressure-sensitive adhesive structure of the present invention is preferably produced by the method for producing a pressure-sensitive adhesive structure of the present invention.
[0091] The method for manufacturing an adhesive structure of the present invention comprises: discharging an adhesive portion forming ink for forming an adhesive portion to be bonded to a contact object from a nozzle, patterning the adhesive portion, and discharging a low elastic portion forming ink for forming a low elastic portion from a nozzle, the low elastic portion having an elastic modulus lower than that of the adhesive portion, patterning the low elastic portion. Optionally, it may include discharging a heat conductive portion forming ink for forming a heat conductive portion from a nozzle to continuously form the heat conductive portion in the thickness direction of the adhesive structure, and may also optionally include other steps. Patterning may be performed in at least one of the discharging of the adhesive portion forming ink and the discharging of the low elastic portion forming ink.
[0092] In the gazette of Japanese Unexamined Patent Application No. 2011-084743, in order to take into account both stress relaxation achieved by lowering the elastic modulus at room temperature (specifically, suppressing the generation of cracks during reflow and damage in temperature cycle tests) and heat resistance and moisture resistance achieved by increasing the peel strength at high temperatures and the elastic modulus at high temperatures, the following technology is proposed: using an epoxy resin, a curing agent, and a polymer compound that is incompatible with the epoxy resin, a phase-separated island structure of an adhesive portion composed of the epoxy resin and the polymer compound having stress relaxation properties is formed during curing heating, thereby improving heat resistance reliability.
[0093] However, in the technology of the present invention, since the adhesive material and the low-elastic material are mixed roughly uniformly in the adhesive layer, there is a problem that the combination cannot be adjusted in the thickness direction (inside the film) and the planar direction (direction roughly perpendicular to the thickness) of the adhesive layer to take into account both adhesion and stress relaxation.
[0094] In addition, in the previous chip bonding components, there is a problem that it is difficult to cope with the increase in heat generation of semiconductors and the thin filmization of semiconductor packages. Specifically, due to the increase in heat generation caused by highly integrated chips and the thinning of devices such as smart phones, chip bonding components are required to be highly heat-resistant and thin-filmed. If the film is thinned, the stress relaxation performance is easily reduced, and the adhesive is easily peeled off from the periphery due to warping. In addition, in the lead part of wire bonding, flip chip, etc., the adhesive layer is not filled sufficiently, so bubbles or gaps are easily generated, and there is a problem of reduced bonding strength.
[0095] In the sheet-like adhesive layer, if it is filmized (for example, below 50 μ m), it is difficult to operate and easily reduces production efficiency. In addition, due to the use of materials with low thermal conductivity such as resin, it is also difficult to filmize, so it is difficult to improve the thermal conductivity (heat dissipation) characteristics between the upper and lower adhesive layers. In addition, when applied as a paste, it is generally applied by a dispenser, but the film of this coating method is difficult to be coated evenly. However, if an immiscible polymer compound is mixed in epoxy resin, the viscosity of the ink increases, so it is difficult to adopt a coating method other than the distribution method. Therefore, if ceramics or metal fillers are added in order to impart thermal conductivity or reduce the linear thermal expansion coefficient, there is a problem that the viscosity is easily further increased and the coating property deteriorates.
[0096] In contrast, the adhesive structure of the present invention can adjust the configuration by forming the adhesive portion and the low elastic portion into a patterned structure, so that the configuration of each component can be configured to obtain excellent adhesiveness and heat resistance, and reduce the deformation amount in the thickness direction (in the film) and the plane direction (direction substantially perpendicular to the thickness direction), so that the film has excellent stress relaxation performance while having adhesiveness and heat resistance. In other words, by configuring the low elastic portion in a manner that reduces the deformation amount in the film and in the plane to relax the stress of the adhesive structure, even a thin film can obtain excellent adhesiveness, heat resistance and stress relaxation performance.
[0097] In addition, in the method for manufacturing the adhesive structure of the present invention, by using different inks to form the adhesive portion and the low elastic portion, the range of ink material selection can be expanded, and the ink viscosity can be reduced without adding a solvent. By reducing the viscosity of the ink, the thin film coating and filling performance of the adhesive structure can be improved, and the patterning accuracy using the inkjet method can be improved, and the generation of bubbles and voids can be reduced.
[0098] In particular, by using an inkjet method to apply the adhesive portion and the low elastic portion, it is possible to form an arbitrary pattern and an adhesive structure having excellent film uniformity, which is preferred. In addition, the use of low-viscosity ink can achieve excellent filling properties in wiring portions such as wire bonding and flip chips while also allowing pattern coating, which is also advantageous in that the generation of bubbles or voids that become the starting point of peeling of the adhesive structure can be suppressed.
[0099] The following is a description of the adhesive structure of the present invention and a method for manufacturing the adhesive structure of the present invention. The present invention includes but is not limited to the embodiments shown below. Within the scope that the inventors can think of, the embodiments can be modified by addition, correction, deletion, etc. to form other embodiments. However, as long as the functions and effects of the present invention can be exerted, any form is included in the scope of the present invention.
[0100] In the adhesive structure, the adhesive portion is formed in a manner that is at least bonded to the contact surface of the contact object, and preferably has the performance of maintaining adhesiveness even at high temperatures. In addition, the low elastic portion has the performance of relieving thermal stress (deformation), and is preferably easy to stretch. In addition, by making at least any one of the adhesive portion and the low elastic portion have a patterned shape formed by patterning, the adhesive performance and thermal stress relaxation performance can be optimized at various parts of the adhesive structure. Therefore, the adhesive structure has excellent heat resistance that takes into account both adhesiveness and stress relaxation characteristics at high temperatures.
[0101] In this specification, the term "patterning" refers to at least one of the following: forming a sparse distribution of the adhesive portion and the low elastic portion in at least any one direction of the thickness direction and the plane direction (the direction substantially perpendicular to the thickness direction) of the adhesive structure; in the adhesive structure, the adhesive portion and the low elastic portion are intentionally (artificially) formed into a desired shape. Therefore, the "patterning" does not include an unintentional (naturally occurring) island structure formed into an arbitrary shape. This is due to the manufacturing method of the adhesive structure, and the patterned shape can be achieved by the manufacturing method of the adhesive structure.
[0102] The patterning method is not particularly limited, and may be any one of a method of forming the low elastic portion in a gap of the adhesive portion by patterning or a method of forming the adhesive portion in a gap of the low elastic portion by patterning.
[0103] In addition, when the adhesive structure has other parts (for example, a heat conducting part, etc.) in addition to the adhesive part and the low elastic part, as the method of patterning, a method of forming the low elastic part and the other parts in the gap of the adhesive part formed by patterning, a method of forming the adhesive part in the gap of the low elastic part and the other parts formed by patterning, etc., can be cited. There is no particular restriction on the order of patterning the low elastic part and the other parts. Therefore, in the method for manufacturing the adhesive structure, there is no particular restriction on the order of the adhesive part forming process, the low elastic part forming process and the heat conducting part forming process. In addition, each of these processes can be performed independently or simultaneously.
[0104] The adhesive portion is formed by discharging the adhesive portion forming ink from the nozzle, but the adhesive portion forming ink may be formed by overlapping the landed droplets to form a thick film. In this case, the adhesive portion forming ink, the low elastic portion forming ink for forming the low elastic portion, or the heat conductive portion forming ink for forming the heat conductive portion described later may be layered alone, or two or more inks selected from the adhesive portion forming ink, the low elastic portion forming ink, and the heat conductive portion forming ink may be alternately landed and layered.
[0105] As the coating method for patterning the bonding portion, the low elastic portion, and the optional heat conducting portion, there is no particular limitation, and it can be appropriately selected from known methods, for example, including but not limited to spin coating, casting, micro gravure coating, rod coating, roller coating, wire rod coating, dip coating, slit coating, capillary coating, inkjet, spray coating, nozzle coating, dispenser coating, gravure coating, screen printing, flexographic printing, offset printing, reverse printing, etc. Among them, it is preferred not to use a printing plate, a spray coating, a dispenser coating, and an inkjet method that can form a coating film in a non-contact manner. By these coating methods, it is possible to carry out coating on demand consistent with the pattern. From the viewpoint of being able to form a high-precision pattern, an inkjet method is particularly preferred, and it is more preferred that at least any one of the bonding portion and the low elastic portion is formed by an inkjet method.
[0106] In order to improve the pattern accuracy of the adhesive portion, the low elastic portion, and the optional thermal conductive portion, it is preferred to use a method of patterning while photocuring at least the adhesive portion, the low elastic portion, or the thermal conductive portion. That is, by the method, the patterned droplets are photocured for a period of time before the droplets expand using the ink for forming the adhesive portion, the ink for forming the low elastic portion, or the ink for forming the thermal conductive portion, thereby improving the formation accuracy of the pattern. The adhesion of the adhesive surface (the droplets on the outermost layer) during bonding can be maintained by adopting any one of the following three methods: a method of forming a semi-cured state during photocuring; a method of stacking photocured droplets so that only the droplets on the outermost layer of the adhesive structure on the contact surface of the contact object are not photocured; a method of making the cured product after photocuring have adhesion.
[0107] In particular, by mounting an array of UV LEDs on an inkjet printing system with a nozzle, the UV LEDs can be used to instantly cure the ejected droplets, thereby enabling high-precision patterning.
[0108] In the inkjet method, dispenser coating method or spray coating method, a pattern can be formed without using a plate, and the adhesive portion can be directly coated on the contact object, so compared with the method of cutting and pasting a pre-made adhesive structure, the adhesive structure can be formed in a thin film and the production efficiency is high. The inkjet method is a particularly preferred coating method because it is excellent in fine pattern formation and film thickness uniformity.
[0109] By changing the patterning ratio and configuration of the adhesive portion and the low elastic portion in the adhesive structure, the required adhesiveness and stress relaxation performance can be adjusted according to the contact object. That is, in general, the stress (deformation) of the adhesive structure is uneven in the thickness direction and the plane direction, therefore, the adhesive portion and the low elastic portion are formed by patterning, and the stress relaxation performance is improved. In particular, since the stress caused by the difference in linear thermal expansion coefficient of the adhesive object (for example, chip or substrate) is easily concentrated on the peripheral end of the planar direction (with the direction of the adhesive surface of the contact object), it is preferred to pattern the volume ratio (low elastic portion / adhesive portion) of the volume of the low elastic portion relative to the volume of the adhesive portion at the peripheral end in a larger manner than the central portion of the planar direction of the adhesive structure.
[0110] On the other hand, from the viewpoint of adhesion to the contact object, the adhesive structure may be patterned so that the outer peripheral end in the planar direction becomes the adhesive portion.
[0111] In the adhesive structure, the shape and size of the adhesive portion and the low elastic portion exposed on one surface may be the same as or different from the shape and size of the adhesive portion and the low elastic portion exposed on the other surface.
[0112] For example, the peripheral shape of the low elastic part surrounded by the adhesive part and / or the peripheral shape of the low elastic part surrounded by the adhesive part is not particularly limited and can be appropriately selected according to the purpose, for example, a combination of straight lines, circular arcs and elliptical arcs can be cited. Specific examples of the combination of shapes include dot-shaped, linear, ring-shaped, lattice-shaped, radial, circular, quadrilateral, fan-shaped, cylindrical, conical, etc. (see Figure 4A to Figure 4H ).
[0113] In addition, the low elasticity portion may not be exposed on the surface of the adhesive structure. That is, the low elasticity portion may be patterned in the thickness direction or plane direction of the adhesive structure (in the direction that is not exposed on the surface of the adhesive structure and is approximately perpendicular to the cross section in the thickness direction). At this time, the peripheral shape of the low elasticity portion surrounded by the adhesive portion is not particularly limited and can be appropriately selected according to the purpose. For example, a combination of straight lines, circular arcs and elliptical arcs can be cited. Specific examples of the combination shape include dot-shaped, linear, ring-shaped, lattice-shaped, radial, circular, quadrilateral, fan-shaped, cylindrical, conical, etc. (refer to Figure 3A to Figure 3I ).
[0114] The shape of the adhesive structure can be confirmed by mapping analysis in the cross-sectional direction and the planar direction using Fourier transform infrared spectroscopy (FT-IR) or the like.
[0115] The shape of the adhesive structure is not particularly limited as long as the adhesive portion and the low elastic portion are patterned, and can be appropriately selected depending on the purpose, and may be in a layered form or a bulk form.
[0116] In this specification, the term "laminated" means that the thickness is less than 1,000 μm, and "block-shaped" means that the thickness exceeds 1,000 μm. These shapes can be appropriately selected according to the target use form. For example, in the bonding of a semiconductor (chip) requiring thin filmization and various materials bonded to the semiconductor (chip), a laminated adhesive structure can be preferably used.
[0117] When the adhesive structure is layered, as its thickness, it is less than 1000 μ m, preferably 1 μ m to 500 μ m, and from the viewpoint of thinning requirements and reducing thermal resistance, it is more preferably 1 μ m to 50 μ m. The thickness of the adhesive structure can be measured using a probe meter (Alpha-Step D-500, KLA-Tenchore), an optical reflectometer (F50 File Metrics), etc. In addition, in this specification, the term "thickness" refers to measuring any three places with the probe meter, and calculating the "average thickness" of the average value.
[0118] <Adhesive Section and Adhesive Section Forming Step>
[0119] The adhesive portion is a member capable of adhering to a contact object. The adhesive portion is preferably formed by the adhesive portion forming step.
[0120] The adhesive portion forming step is a step of discharging an adhesive portion forming ink for forming an adhesive portion capable of adhering to a contact object from a nozzle to form the adhesive portion.
[0121] The contact object is not particularly limited and may be appropriately selected depending on the purpose. Examples thereof include a heating element, a cooling element, a substrate, and an electrode.
[0122] The material forming the adhesive portion is not particularly limited and may be appropriately selected depending on the purpose. From the viewpoint of obtaining mechanical adhesive strength, it preferably contains a resin having an adhesive function and further contains other materials as necessary.
[0123] Resin
[0124] As the resin with bonding function, there is no particular restriction, and can be suitably selected according to purpose, for example, light-curable resin, thermosetting resin etc. can be enumerated. These can be used alone, and also can be used in combination with other. Particularly, under the situation that the light transmittance of the bonding surface of the bonding portion and the contact object is not suitable for penetrating the contact object and carrying out photocuring, preferably the bonding portion contains thermosetting resin at least. In addition, preferably at least any one of the bonding portion and the low elasticity portion contains light-curable resin.
[0125] Specific examples of the resin include, but are not limited to, polyurethane resins, epoxy resins, phenolic resins, polyimide resins, ester resins, vinyl resins, silicone resins, styrene resins, cellulose resins, amide resins, (meth) acrylic resins, melamine resins, fluorine resins, etc. These can be used alone or in combination with others. Among them, epoxy resins, silicone resins, and polyimide resins are preferred as the resins because of their good heat resistance, and epoxy resins are more preferred because of their small curing shrinkage.
[0126] The adhesive portion may be formed by using an adhesive portion forming ink containing a monomer component of the resin, applying the adhesive portion forming ink onto the contact object, and causing a polymerization reaction to occur.
[0127] 《Adhesion forming ink》
[0128] The adhesive portion forming ink may contain the resin, or may contain a monomer component of the resin and a polymerization initiator, and may optionally contain other components. From the viewpoint of enabling good patterning, it preferably contains a monomer component of the resin and a polymerization initiator.
[0129] -Monomer components-
[0130] There are no particular restrictions on the monomer components of the resin, and they can be appropriately selected according to the type of resin used, for example, epoxy monomers, (meth)acrylate monomers, oxetane monomers, urethane monomers, silicone monomers, etc. These can be used alone or in combination with others. Among them, as the monomer component of the resin, it is preferred to contain epoxy monomers. In the present invention, "(meth)acrylate monomers" are a general term for "acrylate monomers" and "methacrylate monomers".
[0131] --Epoxy Monomer--
[0132] The epoxy monomer is not particularly limited and may be appropriately selected depending on the intended purpose. Examples of the epoxy monomer include alicyclic epoxy monomers, glycidyl ether epoxy monomers, and glycidyl amine epoxy monomers.
[0133] The alicyclic epoxy monomer has a high glass transition temperature (Tg) due to its ring structure, and has excellent heat resistance, while the monomer viscosity is low.
[0134] The glycidyl ether type epoxy monomer can easily adjust the elastic modulus of the cured product to a low elasticity, and the monomer viscosity is low.
[0135] The glycidylamine type epoxy monomer easily obtains adhesive strength.
[0136] By mixing various epoxy monomers having the above characteristics, it is possible to use the adhesive portion forming ink suitable for the inkjet method.
[0137] The alicyclic epoxy monomer includes, but is not limited to, a compound represented by any one of the following structural formulas 1 to 16. These may be used alone or in combination with other compounds.
[0138] [Chemical formula 1]
[0139]
[0140] Wherein, in the structural formula 15, n represents an integer of 1 or 2.
[0141] The alicyclic epoxy monomer may be appropriately synthesized, or a commercially available product may be used.
[0142] Commercially available products of the alicyclic monomer include, but are not limited to, EPOCALIC THI-DE, EPOCALIC DE-102, EPOCALIC DE-103, VNBB-ME (all manufactured by ENEOS), DCPD-DE (manufactured by Japan Materials Technology Co., Ltd.), Celloxide (CEL) 8010P, CEL2010P, CEL2081, CEL2000 (all manufactured by Daicel), etc.
[0143] Examples of glycidyl ether epoxy monomers include, but are not limited to, allyl diglycidyl ether and bisphenol diglycidyl ether. Specific examples include compounds represented by any one of the following structural formulas 17 to 24. These can be used alone or in combination with other compounds.
[0144] [Chemical formula 2]
[0145]
[0146] (Wherein, in the structural formula 17, n represents 12. In the structural formula 19, n represents 9.
[0147] The glycidyl ether type epoxy monomer may be appropriately synthesized, or a commercially available product may be used.
[0148] Commercially available products of the glycidyl ether type epoxy monomer include, but are not limited to, Rikaresin DME-100 (manufactured by Shin Nippon Chemical Co., Ltd.), Epolight M-1230, Epolight 40E, Epolight 100E, Epolight 200E, Epolight 400E, Epolight 70P, Epolight 200P, Epolight 400P, Epolight 1500NP, Epolight 1600, Epolight 80MF, and Epolight 100MF (manufactured by Kyoeisha Chemical Co., Ltd.), Shofree (registered trademark) PETG, Shofree (registered trademark) BATG (manufactured by Showa Denko K.K.), Denacol EX-614B, Denacol EX-313, Denacol EX-512, Denacol EX-321, Denacol EX-321L, Denacol EX-612, Denacol EX-614, Denacol EX-622, Denacol EX-314, Denacol EX-421, Denacol EX-521, Denacol EX-411, Denacol EX-171, Denac o lEX-146, Denacol EX-121, Denacol EX-141, Denacol EX-145, Denacol EX-147, Denacol EX-192, Denacol EX-731 (all manufactured by Nagase ChemteX), YL9028 (manufactured by Mitsubishi Chemical Corporation), OCR-EP, NPG(D), DY-BP, DY-BP (all manufactured by Yokkaichi Synthetic Co., Ltd.), etc.
[0149] The glycidylamine type epoxy monomer has an amine structure.
[0150] The glycidylamine type epoxy monomer may be appropriately synthesized, or a commercially available product may be used.
[0151] Commercially available products of the glycidylamine-based epoxy monomer include, but are not limited to, TETRAD-X (manufactured by Mitsubishi Gas Chemical Co., Ltd.) and VH-523 (manufactured by Nippon Steel Chemicals & Materials Co., Ltd.).
[0152] --(Meth)acrylate monomers--
[0153] The (meth)acrylate monomer is not particularly limited and can be appropriately selected from common photopolymerizable (meth)acrylate monomers according to the intended purpose. These may be used alone or in combination with other monomers.
[0154] The (meth)acrylate monomer may be appropriately synthesized, or a commercially available product may be used.
[0155] Commercially available products of the (meth)acrylate monomer include, but are not limited to, AOMA (registered trademark) (manufactured by Nippon Shokubai Co., Ltd.), HEA (hydroxyethyl acrylate), HPA (hydroxypropyl acrylate), 4-HBA (4-hydroxybutyl acrylate), AIB (isobutyl acrylate), TBA (tert-butyl acrylate), NOAA (n-octyl acrylate), INAA (isononyl acrylate), Viscoat #197 (nonyl acrylate), IDAA (nonyl acrylate), LA (lauryl acrylate), STA (stearyl acrylate), ISTA (isostearyl acrylate), IBXA (isobornyl acrylate), and Viscoat #155 (cyclohexyl acrylate). 、Viscoat#196(3,3,5-trimethylcyclohexyl acrylate), Viscoat#160(benzyl acrylate), Viscoat#192(phenoxyethyl acrylate), Viscoat#150(tetrahydrofuran acrylate), Viscoat#190(carbitol acrylate), 2-MTA(methoxyethyl acrylate), Viscoat#MTG(methoxytriethylene glycol acrylate), MPE400A(methoxypolyethylene glycol acrylate), MPE550A(methoxypolyethylene glycol acrylate), OXE-10(3-ethyl-3-(acryloyloxymethyl)oxetane), OXE-30(methacrylic acid oxetane ester), MEDOL-10 (3-ethyl-3-(acryloyloxymethyl)oxetane), Viscoat #200 (cyclotrimethylolpropane formal acrylate) (all manufactured by Osaka Organic Chemical Industry Co., Ltd.), A-LEN-10 (ethoxylated o-phenylphenol acrylate), AM-90G (ethoxylated o-phenylphenol acrylate), AM-130G (ethoxylated o-phenylphenol acrylate), AMP-20GY (ethoxylated o-phenylphenol acrylate), A-SA (2-acryloyloxyethyl succinic acid), 701A (propyl acrylate 2-hydroxy-3-methacrylate), A-200 (polyethylene glycol #200 dimethacrylate), acrylate), A-400 (polyethylene glycol #400 diacrylate), A-600 (polyethylene glycol #600 diacrylate), A-100 (polyethylene glycol #100 diacrylate), ABE-300 (ethoxylated bisphenol-A diacrylate), A-BPE-10 (ethoxylated bisphenol-A diacrylate), A-BPE-20 (ethoxylated bisphenol-A diacrylate), A-BPE-4 (ethoxylated bisphenol-A diacrylate), A-DCP (tricyclodecane dimethanol diacrylate), A-DOD-N (1,10-decanediol diacrylate), A-HD-N (1,6-hexanediol diacrylate), A-N0D-N (1,6-hexanediol diacrylate), APG-200 (tripropylene glycol diacrylate), APG-400 (polypropylene glycol #400 diacrylate), APG-700 (polypropylene glycol #700 diacrylate), A-PTMG-65 (polytetramethylene glycol #650 diacrylate), A-9300 (polytetramethylene glycol #650 diacrylate), A-GLY-9E (ethoxylated glyceryl triacrylate), A-GLY-20E (ethoxylated glyceryl triacrylate), A -TMM-3 (pentaerythritol tri- and tetraacrylate), A-TMM-3L (pentaerythritol tri- and tetraacrylate), A-TMPT (trimethylolpropane triacrylate), AD-TMP (ditrimethylolpropane tetraacrylate), ATM-35E (ethoxylated pentaerythritol tetraacrylate), A-TMMT (pentaerythritol tetraacrylate), A-9550 (dipentaerythritol polyacrylate), A-DPH (dipentaerythritol polyacrylate) (all manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), etc.
[0156] --Oxetane Monomer--
[0157] The oxetane monomer is not particularly limited and can be appropriately selected according to the purpose, including but not limited to the compounds represented by any one of the following structural formulas 25 to 33. These can be used alone or in combination with others.
[0158] [Chemical formula 3]
[0159]
[0160] In structural formula 32, n represents an integer of 1 or 2.
[0161] The oxetane monomer may be appropriately synthesized, or a commercially available product may be used.
[0162] Commercially available products of the oxetane monomer include, but are not limited to, ARON OXETANE OXT101, ARON OXETANE OXT212, ARON OXETANE OXT121, ARON OXETANE OXT221 (all manufactured by Toagosei Co., Ltd.), ETERNACOLL (registered trademark) HBOX, ETERNACOLL (registered trademark) OXBP, ETERNACOLL (registered trademark) OXIPA (all manufactured by Ube Industries, Ltd.), and the like.
[0163] --Urethane Monomer--
[0164] The urethane monomer is not particularly limited and can be appropriately selected from common urethane monomers according to the purpose. These may be used alone or in combination with other monomers.
[0165] The urethane monomer may be appropriately synthesized, or a commercially available product may be used.
[0166] Commercially available products of the urethane monomer include, but are not limited to, US3003, US3003M, US3007, US3007M, and US3123M (all manufactured by Kyoeisha Chemical Co., Ltd.).
[0167] --Organic Silicone Monomer--
[0168] The organosilicon monomer is not particularly limited and can be appropriately selected from common organosilicon monomers according to the purpose, for example, organosilicon compounds having reactive groups at one or both ends of polydimethylsiloxane, etc. These can be used alone or in combination with others.
[0169] The organosilicon monomer may be appropriately synthesized, or a commercially available product may be used.
[0170] Commercially available products of the silicone monomer include, but are not limited to, Silaplane (registered trademark) FM-3311, Silaplane (registered trademark) FM-3321, Silaplane (registered trademark) FM-3325 (all manufactured by JNC Corporation), STP-103-UV, STP-104-UV (all manufactured by Shin-Etsu Silicone Co., Ltd.), and the like.
[0171] The adhesive portion forming ink preferably contains the epoxy monomer as described above. The content of the epoxy monomer in the adhesive portion forming ink is not particularly limited and can be appropriately selected according to the purpose, but is preferably 40% by mass or more, more preferably 50% by mass or more relative to the total mass of the adhesive portion forming ink. If the content of the epoxy monomer is 40% by mass or more, curing shrinkage is small and heat resistance is excellent, so it is preferred.
[0172] When the monomer component in the adhesive portion forming ink is a mixture of the epoxy monomer and a monomer component other than the epoxy monomer, the content of the monomer other than the epoxy monomer is not particularly limited and can be appropriately selected according to the purpose, preferably 5% to 90% by mass, more preferably 5% to 70% by mass relative to the epoxy monomer. As the monomer component other than the epoxy monomer, an oxetane compound is preferred from the aspects of excellent compatibility with the epoxy monomer and low viscosity.
[0173] -Polymerization initiator-
[0174] The polymerization initiator is not particularly limited and can be appropriately selected from known polymerization initiators, including but not limited to photocationic polymerization initiators, photoradical polymerization initiators, thermal polymerization initiators, etc. These can be used alone or in combination with others.
[0175] --Photocationic polymerization initiator--
[0176] The photocationic polymerization initiator is not particularly limited and can be appropriately selected according to the purpose, including but not limited to photoacid generators such as onium salts with sulfonium ions or iodonium ions as the cation part. Among them, as the photocationic polymerization initiator, a compound with an anion part that is less corrosive to the metal part is preferred. As specific examples of the photocationic polymerization initiator, compounds whose anion part (generated acid) is B(C6F5)4, PF3(C2F5)3, etc. can be cited.
[0177] The photocationic curing initiator may be synthesized as appropriate, or a commercially available product may be used.
[0178] Commercially available products of the photocationic curing initiator include, but are not limited to, CPI (registered trademark) -110P, CPI (registered trademark) -110A, CPI (registered trademark) -210S, CPI (registered trademark) -110B, CPI (registered trademark) -310B, CPI (registered trademark) -410B, CPI (registered trademark) -310FG, IK-1 FG (all manufactured by SAN-APRO Co., Ltd.), etc.
[0179] --Photoradical polymerization initiator--
[0180] The photoradical polymerization initiator is not particularly limited and may be appropriately selected according to the purpose, including but not limited to alkylphenone compounds, acylphosphine oxides, oxyphenylacetic acid ester compounds and the like.
[0181] The photoradical polymerization initiator may be synthesized as appropriate, or a commercially available product may be used.
[0182] Commercially available products of the photoradical polymerization initiator include, but are not limited to, Omnirad 184 (former Irgacure 184), Omnirad 651 (former Irgacure 651), Omnirad 1173 (former Irgacure 1173), Omnirad 2959 (former Irgacure 2959), Omnirad 369 (former Irgacure 369), Omnirad 907 (former Irgacure 907), Omnirad BMS, Omnirad DETX, Omnirad TPO H (former Irgacure TP 0), Omnirad 819 (former Irgacure 819) (all manufactured by IGM Resins BV), Irgacure OXE01, Irgacure OXE02, Irgacure OXE03, Irgacure OXE 04 (all manufactured by BASF JAPAN) and the like.
[0183] --Thermal polymerization initiator--
[0184] The thermal polymerization initiator is not particularly limited and may be appropriately selected depending on the intended purpose, including but not limited to photoacid generators such as onium salts having a sulfonium ion or an iodonium ion as a cation portion.
[0185] The thermal polymerization initiator may be appropriately synthesized, or a commercially available product may be used.
[0186] Examples of commercially available products of the thermal polymerization initiator include, but are not limited to, SAN-AID SI-60L, SAN-AID SI-80L, SAN-AID SI-100L, SAN-AID SI-110 and L SAN-AID SI-150 (all manufactured by Sanshin Chemical Industries, Ltd.), TA-100, TA-100 FG, IK-1 and IK-1 FG (all manufactured by SAN-APRO), Omnicat 250 (former Irgacure 250) and Omnicat 270 (former Irgacure 270) (all manufactured by IGM Resins BV), and the like.
[0187] The content of the polymerization initiator in the ink for forming the bonding portion is not particularly limited and can be appropriately selected according to the purpose, but is preferably 0.1% to 10% by mass, more preferably 0.2% to 2% by mass, relative to the total mass of the ink for forming the bonding portion. When the content of the polymerization initiator is 0.1% to 10% by mass, the curing reaction can be properly completed and the unreacted portion is less likely to remain as reactive impurities.
[0188] -Other ingredients-
[0189] The other components in the adhesive portion forming ink are not particularly limited and can be appropriately selected according to the purpose, and examples thereof include inorganic particles, resins or resin particles, adhesion improvers, solvents, etc. These can be used alone or in combination with other components.
[0190] --Inorganic particles--
[0191] The inorganic particles are added to reduce the linear thermal expansion coefficient of the bonding portion and to improve the film strength.
[0192] There is no particular restriction as the inorganic particles and may be appropriately selected according to purpose, and examples thereof include, but are not limited to, ceramic materials, magnetic particles and the like.
[0193] Examples of the ceramic material include, but are not limited to, silicon dioxide (SiO2), aluminum oxide (Al2O3), aluminum nitride (AlN), boron nitride (BN), etc. Compared with resin materials, the ceramic material has a smaller linear thermal expansion coefficient and a higher softening temperature, so it is possible to reduce the linear thermal expansion coefficient of the bonding portion and improve the film strength under high temperature conditions. The magnetic particles include, for example, but are not limited to iron (Fe), nickel (Ni), cobalt (Co), etc. The magnetic particles can be given the function of shielding electromagnetic waves. These can be used alone or in combination with others.
[0194] The inorganic particles may be synthesized as appropriate, or commercially available particles may be used.
[0195] Commercially available products of the inorganic particles include, for example, but are not limited to AEROSIL (registered trademark) OX50, AEROSIL (registered trademark) 50, AEROSIL (registered trademark) 90G, AEROSIL (registered trademark) 130, AEROSIL (registered trademark) 150, AEROSIL (registered trademark) 200, AEROSIL (registered trademark) 300, AEROSIL (registered trademark) 380, AEROSIL (registered trademark) RM50, AEROSIL (registered trademark) R711, AEROSIL (registered trademark) R7200, AEROXIDE (registered trademark) P25, AEROXIDE (registered trademark) P90 AluC (all manufactured by AEROSIL Co., Ltd. of Japan), Seahostar (registered trademark) KE-S10, Seahostar (registered trademark) S30, Seahostar (registered trademark) S50 (all manufactured by Nippon Shokubai Co., Ltd.), etc.
[0196] The content of the inorganic particles in the ink for forming the bonding portion is not particularly limited and can be appropriately selected according to the purpose. It is preferably 10% to 70% by mass, and more preferably 10% to 50% by mass, relative to the total mass of the ink for forming the bonding portion. When the content of the inorganic particles is 10% by mass or more, the effects of linear thermal expansion and film strength are easily obtained, and when it is 50% by mass or less, the bonding portion is not easy to become brittle and the ink viscosity is not easy to increase, so it is preferred.
[0197] --resin or resin particles--
[0198] The resin or resin particles are added to give the adhesive part flexibility and relieve thermal stress. There are no special restrictions on the resin or resin particles, and they can be appropriately selected according to the purpose. Preferably, the material is a linear polymer with at least any one of low elasticity and softness, such as but not limited to styrene butadiene resin, acrylonitrile butadiene resin, (meth) acrylic resin, epoxy resin, etc. These can be used alone or in combination with others. In addition, it can also be a core-shell type multilayer structure polymer particle in which a rubber-like polymer is configured inside an acrylic copolymer. Among them, as the resin or resin particles, styrene butadiene resin and acrylic resin are preferred. In order to relieve thermal stress, the resin or resin particles have a low glass transition temperature (Tg), Tg is about 30°C or less, close to room temperature, and therefore are preferred.
[0199] Here, the resin or resin particles being "low elastic" means, for example, a material having an elastic modulus of 200 MPa or less. In addition, the resin or resin particles being "flexible" means, for example, a material having an elastic deformation rate of 70% or more. The elastic deformation rate of the resin and resin particles can be confirmed, for example, by measuring the indentation elastic modulus using a microhardness meter (e.g., FISCHERSCOPE (registered trademark) HM2000, manufactured by Fischer Instruments).
[0200] The resin material with low elasticity can be appropriately synthesized or a commercial product can be used. Commercial products of the resin material with low elasticity include, but are not limited to, ARUFON (registered trademark) US-1000, ARUFON (registered trademark) UH-2000, ARUFON (registered trademark) UC-3000, ARUFON (registered trademark) UG-4000, ARUFON (registered trademark) UF-5000, ARUFON (registered trademark) US-600, etc.
[0201] The resin particles having low elasticity may be synthesized as appropriate, or commercially available products may be used. Examples of commercially available products of the resin particles having low elasticity include, but are not limited to, Kane Ace (registered trademark) MX-150, Kane Ace (registered trademark) MX-553 (manufactured by Kaneka Co., Ltd.), Finesphere (registered trademark) MG-155, Finesphere (registered trademark) MG-351, Finesphere (registered trademark) MG-451, Finesphere (registered trademark) MG-651, Finesphere (registered trademark) PZP-1003, Finesphere (registered trademark) BGK-001 (manufactured by Nippon Paint Industrial Coatings Co., Ltd.), Metablen (registered trademark) C-223A, Metablen (registered trademark) C-215A-201A, Metablen (registered trademark) C-140A, Metablen (registered trademark) E-860A, Metablen (registered trademark) E-870A, Metablen (registered trademark) E-875A, Metablen (registered trademark) Metablen (registered trademark) W-300A, Metablen (registered trademark) W-450A, Metablen (registered trademark) W-600A, Metablen (registered trademark) W-377, Metablen (registered trademark) S-2002, Metablen (registered trademark) S-2006, Metablen (registered trademark) S-2501, Metablen (registered trademark) S-2030, Metablen (registered trademark) S-2100, Metablen (registered trademark) S-2200, Metablen (registered trademark) SRK200A, Metablen (registered trademark) SX-006, Metablen (registered trademark) SX-00 (all manufactured by Mitsubishi Chemical Corporation), Zefiac F351, Staphyloid AC-3355, AC-3816N, AC-3832SD, AC-4030 and AC-3388 (all manufactured by Aica Industries, Ltd.), etc.
[0202] The content of the resin or resin particles in the ink for forming the bonding portion is not particularly limited and can be appropriately selected according to the purpose. It is preferably 1% to 50% by mass, and more preferably 3% to 20% by mass relative to the total mass of the ink for forming the bonding portion. When the content of the resin or resin particles is 1% by mass or more, thermal stress can be further appropriately relaxed. In addition, if the content of the resin or resin particles is 50% by mass or less, the increase in viscosity of the ink for forming the bonding portion can be suppressed, so it can be suitable for inkjet method. If it is 50% by mass or less, it is difficult to become the cause of bubbles or voids at high temperatures.
[0203] --Close contact improver--
[0204] The adhesion improver is a compound composed of organic matter and silicon. Silane coupling agents having two or more different reactive groups in the molecule can improve the adhesion with the contact object (especially semiconductors and semiconductor substrates), so they are particularly preferred. The adhesion improver can use commercial products, as specific examples thereof, including but not limited to DOWSIL Z-6040, DOWSIL Z-6062 (the above are made by DOW), KMB-403 (made by Shin-Etsu Silicone Co., Ltd.), etc.
[0205] The content of the adhesion improving agent in the adhesive portion forming ink is not particularly limited and can be appropriately selected according to the purpose. It is preferably 0.1% to 20% by mass, and more preferably 0.1% to 5% by mass, relative to the total mass of the adhesive portion forming ink. If the content of the adhesion improving agent is 0.1% by mass or more, a adhesion effect can be obtained. In addition, if the content of the adhesion improving agent is 20% by mass or less, it is preferred to suppress the reduction of ink strength.
[0206] --Solvents--
[0207] The solvent is not particularly limited and can be appropriately selected according to the purpose, including, but not limited to, terpineol, 1-methoxy-2-propanol, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, 2-methoxyethyl acetate, 2-methoxybutyl acetate, 2-butanone, etc. These can be used alone or in combination with others.
[0208] The content of the solvent in the ink for forming the bonding part is not particularly limited and can be appropriately selected according to the purpose, but if the viscosity of the ink for forming the bonding part is appropriate, it is preferably not contained. When the solvent is added, it is preferably 1% to 30% by mass, and more preferably 1% to 5% by mass, relative to the total mass of the ink for forming the bonding part. If the content of the solvent is 1% by mass or more, the management of the solvent component of the ink for forming the bonding part becomes easy, and the viscosity can be reduced, so that it is suitable for inkjet printing. If it is less than 30% by mass, it is difficult to cause bubbles or voids at high temperatures.
[0209] Among them, the adhesive portion forming ink is preferably a photocurable composition, and more preferably contains the epoxy monomer and the photocationic polymerization initiator or the photoradical polymerization initiator.
[0210] The viscosity of the adhesive portion forming ink is not particularly limited and can be appropriately selected according to the purpose, but is preferably a low-viscosity ink that can be ejected from a nozzle of a small diameter by an inkjet method, preferably 200 mPa·s or less, more preferably 50 mPa·s or less at 25°C. In addition, the lower limit of the viscosity of the adhesive portion forming ink is not particularly limited and can be appropriately selected according to the purpose, but is preferably 5 mPa·s or more at 25°C from the viewpoint of ejectability and molding accuracy.
[0211] The viscosity of the adhesive portion forming ink can be measured by conventional methods, for example, the method described in JIS Z8803 can be used. In addition, for example, a cone-plate type rotational viscometer (for example, VISCOMETER TVE-22L, manufactured by Toki Sangyo Co., Ltd.) can be used, using a conical rotor (1°34'×R24), with a rotation speed of 10 rpm and a constant temperature circulating water temperature of 20°C to 65°C. The circulating water temperature can be adjusted using a circulating thermostatic bath (for example, VISCOMATE VM-150III, manufactured by Toki Sangyo Co., Ltd.).
[0212] As long as the adhesive portion can be bonded to the contact object, the adhesive portion may be provided only on one surface in the planar direction of the bonding structure, or may be provided on both surfaces at the same time. The adhesive portion is patterned on the portion of the bonding surface with the contact object where the low elastic portion is not formed. In addition, in the case where the adhesive structure has the thermal conductive portion, the adhesive portion is patterned on the portion of the bonding surface with the contact object where the low elastic portion and the thermal conductive portion are not formed. In addition, in the case where the adhesive structure has a wiring portion such as a wire bonding or a flip chip, the adhesive portion may not be formed in the area where the wiring portion is formed.
[0213] In the adhesive structure, the size in the plane direction of the adhesive portion is not particularly limited and can be appropriately selected according to the purpose, but in order to obtain bonding force, it is preferably more than the thickness of the adhesive structure consisting of the adhesive portion and the low elastic portion. As the size in the plane direction of the adhesive portion in the adhesive structure, it is preferably more than 10 μ m, more preferably more than 100 μ m. When the size in the plane direction of the adhesive portion in the adhesive structure is more than 10 μ m, it is easy to obtain bonding force. In addition, from the viewpoint of stress relaxation characteristics, the size in the plane direction of the adhesive portion in the adhesive structure is preferably less than 50000 μ m, more preferably less than 30000 μ m.
[0214] As the elastic modulus of the bonding portion, as long as it is larger than the low elastic portion, there is no particular restriction, and it can be appropriately selected according to the purpose, but it is preferably below 10,000MPa, and more preferably below 5000MPa. In addition, from the viewpoint of the intensity of the bonding portion, it is preferred that the elastic modulus of the bonding portion is more than 200MPa. When the elastic modulus of the bonding portion is below 10,000MPa, it is not easy to brittle failure.
[0215] The elastic modulus of the adhesive portion can be measured, for example, using a micro-hardness tester (FISCHERSCOPE (registered trademark) HM2000, manufactured by Fischer Instruments).
[0216] <Low Elasticity Section and Low Elasticity Section Forming Step>
[0217] The low elastic part is a part having a smaller elastic modulus than the adhesive part and being patterned. The low elastic part has the ability to relieve thermal stress by being flexible. The low elastic part is preferably formed by the low elastic part forming step.
[0218] The low elastic portion forming step is a step of ejecting a low elastic portion forming ink from a nozzle for forming a low elastic portion having a smaller elastic modulus than the adhesive portion, thereby patterning and forming the low elastic portion.
[0219] The low elastic portion is patterned together with the adhesive portion and the optional heat conductive portion, and the adhesive portion is not mixed inside the low elastic portion (not an island-in-the-sea structure).
[0220] The material forming the low elastic portion is not particularly limited as long as it has a smaller elastic modulus than the adhesive portion, and may be appropriately selected depending on the purpose, but preferably contains a resin and further contains other materials as necessary.
[0221] Resin
[0222] The resin forming the low elastic portion is not particularly limited and may be appropriately selected depending on the purpose, and includes, but is not limited to, photocurable resins, thermosetting resins, etc. These may be used alone or in combination with other resins.
[0223] When the low elasticity part is formed on the outermost layer of the adhesive structure, it is preferably the same resin as a part of the material of the adhesive part. In particular, when the light transmittance of the adhesive surface between the adhesive part and the contact object is not suitable for light curing of the contact object, it is preferred that the low elasticity part contains at least a thermosetting resin.
[0224] Specific examples of the resin include, but are not limited to, polyurethane resins, epoxy resins, phenolic resins, polyimide resins, ester resins, vinyl resins, silicone resins, styrene resins, cellulose resins, amide resins, (meth) acrylic resins, melamine resins, fluorine resins, etc. These may be used alone or in combination with others.
[0225] Among them, epoxy resin, silicone resin, and polyimide resin are preferred as the resin because of their good heat resistance, and epoxy resin is more preferred because of its small curing shrinkage. The resin forming the low elastic portion is configured to have a lower elastic modulus than the resin forming the adhesive portion by mixing the low elastic portion forming ink described later.
[0226] The low elastic portion may be formed by using a low elastic portion forming ink containing a monomer component of the resin, applying the low elastic portion forming ink before or after patterning the adhesive portion using the patterning method, and causing a polymerization reaction.
[0227] <<<Ink for forming low elastic portion>>>
[0228] The ink for forming the low elastic portion may contain the resin, or may contain a monomer component of the resin and a polymerization initiator, and may optionally contain other components. From the viewpoint of enabling good patterning, it preferably contains a monomer component of the resin and a polymerization initiator.
[0229] About the material of described low elasticity portion forming ink, can use the material same as the material of described bonding portion forming ink, therefore omit explanation.In addition, for the physical properties such as viscosity of described low elasticity portion forming ink except elastic modulus, owing to form ink same as described bonding portion, so omit explanation, but for described low elasticity portion forming ink, also can use commercially available low viscosity epoxy ink, acrylic acid ink etc.As described commercially available ink, for example include but not limited to IJSR4000, IJSR9000 (above by sun ink company system), PR1205, PR1243, PR1258 (above by mutual chemical industry company system), SUN-004, SUN-013, SUN-015, C-202, C-400, E635A, E800D (above by sekisui chemical company system), jSVR (by Dexerials company system) etc.
[0230] The low elastic portion forming ink can form a cured product with lower elasticity and excellent softness than the adhesive portion, depending on the type of ink material used and the mixing ratio. Specifically, as the type of ink material for the low elastic portion forming ink, it is preferred to mix at least one ink selected from glycidyl ether type epoxy monomer, glycidyl amine type epoxy monomer, (methyl) acrylate monomer, oxetane monomer, urethane monomer, the resin or resin particles. In addition, by making the mixing ratio of these materials more than the adhesive portion forming ink, it is easy to prepare an ink with lower elasticity than the cured product of the adhesive portion forming ink. The elastic modulus of the cured ink can be confirmed, for example, by measuring the indentation elastic modulus of the film formed and cured on the glass surface with a micro-hardness meter.
[0231] The volume ratio (low elastic part / adhesive structure) occupied by the low elastic part in the adhesive structure is not particularly limited and can be appropriately selected according to the purpose, but preferably 5 volume % to 90 volume %, more preferably 5 volume % to 50 volume % relative to the total volume of the adhesive structure. If the volume ratio occupied by the low elastic part in the adhesive structure is 5 volume % or more, the stress relaxation property is good, and if it is 90 volume % or less, the adhesion of the adhesive part is good. Thermal stress is easily concentrated at the low elastic part, so it is preferably formed at the end of the adhesive structure.
[0232] The elastic modulus of the low elastic part is not particularly limited as long as it is smaller than that of the bonding part, and can be appropriately selected according to the purpose, but is preferably 70% or less of the elastic modulus of the bonding part, and more preferably 50% or less of the elastic modulus of the bonding part. When the elastic modulus of the low elastic part is 70% or less of the elastic modulus of the bonding part, the stress relaxation property is good.
[0233] The comparison between the elastic modulus of the low elastic part and the elastic modulus of the bonding part is not particularly limited and can be appropriately selected according to the purpose, but the elastic modulus ratio [elastic modulus of the low elastic part / elastic modulus of the bonding part] is preferably 0.01% to 70%, more preferably 0.02% to 60%.
[0234] As the elastic modulus of the low elastic portion, as long as it is less than the bonding portion, there is no particular restriction, and it can be appropriately selected according to the purpose, preferably below 3000MPa, more preferably below 2000MPa. When the elastic modulus of the low elastic portion is below 3000MPa, the stress relaxation characteristics are good. The elastic modulus of the low elastic portion can be measured, for example, with a micro-hardness meter (FISCHERSCOPE (registered trademark) HM2000, Fischer Instruments company system).
[0235] <Heat transfer portion and heat transfer portion forming step>
[0236] The heat-conducting part is a part formed continuously in the thickness direction of the adhesive structure. The heat-conducting part has the performance of conducting heat in the thickness direction. Therefore, in the adhesive structure, the heat-conducting part is formed by patterning, so that the thermal conductivity, heat dissipation and electrical conductivity between the upper and lower parts in the thickness direction of the adhesive structure can be improved. Therefore, when the adhesive structure is used to bond a heating element, a cooling element, an electrode, etc., it is preferred to have the heat-conducting part.
[0237] The heat transfer section is preferably formed by the heat transfer section forming step. The heat transfer section forming step is a step of forming the heat transfer section continuous in the thickness direction of the adhesive structure by ejecting a heat transfer section forming ink for forming the heat transfer section from a nozzle.
[0238] The pattern of the heat conducting part in the adhesive structure is not particularly limited as long as it is continuous in the thickness direction of the adhesive structure, and can be appropriately selected according to the purpose, for example, including but not limited to: a pattern surrounded by the adhesive part, a pattern surrounded by the low elastic part, a pattern between the adhesive part and the low elastic part and surrounded by both, etc. For example, the outer peripheral shape of the heat conducting part surrounded by at least one of the adhesive part and the low elastic part is not particularly limited, and can be appropriately selected according to the purpose, for example, including but not limited to a combination of a straight line, a circular arc, and an elliptical arc, etc.
[0239] In the adhesive structure, the shape and size of the heat conductive portion exposed to one surface may be the same as or different from the shape and size of the heat conductive portion exposed to the other surface.
[0240] 《Ink for forming heat transfer part》
[0241] The material forming the heat conducting portion is not particularly limited and may be appropriately selected depending on the intended purpose, but preferably contains a heat conducting material and optionally further contains other components.
[0242] <<<Thermal Conductive Materials>>>
[0243] There is no particular limitation on the thermally conductive material, and it can be appropriately selected according to the purpose, including but not limited to metal materials, carbon, ceramic materials, etc. The metal material includes, but is not limited to, silver (Ag), copper (Cu), gold (Au), aluminum (Al), etc. The ceramic material includes, but is not limited to, silicon dioxide (SiO2), aluminum oxide (Al2O3), aluminum nitride (AlN) and boron nitride (BN), etc. These can be used alone or in combination with others. Among them, the thermally conductive material is preferably a metal material, and metal nanoparticles are more preferred. The metal material can also be used as a conductive material.
[0244] The primary average particle size of the thermally conductive material in the thermally conductive portion forming ink is not particularly limited and may be appropriately selected depending on the intended purpose, but is preferably 0.01 μm to 100 μm, and more preferably 0.3 μm to 10 μm.
[0245] The primary average particle size of the metal nanoparticles in the ink for forming the heat-conducting portion is not particularly limited and can be appropriately selected according to the purpose, preferably 0.005μm to 1μm, and more preferably 0.005μm to 0.2μm. When the primary average particle size of the metal nanoparticles is 0.005μm to 1μm, when the adhesive structure is used to bond a heating element or a cooling element, the unevenness of the contact surface with the heating element or the cooling element is small, and an integrated high heat-conducting portion with a flat contact surface can be formed. In addition, from the viewpoint of being able to sinter by a relatively low temperature treatment of about 150°C, the primary average particle size of the metal nanoparticles is preferably less than 200nm. In addition, by making the metal nanoparticles have a small particle size, the heat-conducting portion can be thin-filmed, or precisely patterned by inkjet printing and coating with a small diameter nozzle.
[0246] The content of the thermally conductive material in the thermally conductive portion forming ink is not particularly limited and can be appropriately selected according to the purpose, but is preferably 15% to 100% by mass, more preferably 40% to 100% by mass, relative to the total mass of the thermally conductive portion forming ink. When the content of the thermally conductive material in the thermally conductive portion forming ink is in the range of 15% to 100% by mass, high thermal conductivity can be obtained.
[0247] The thickness of the heat conducting portion is basically set to be the same as that of the adhesive portion and the low elastic portion, but the area (volume) of the heat conducting portion is set to the most appropriate value through heat dissipation design. In addition, when carbon nanoparticle ink, graphene ink, etc. are used as the carbon material for coating, the thickness of the heat conducting portion is preferably 1 μm to 300 μm. In addition, when the ceramic material is applied as a ceramic paste mixed with ceramic particles and resin, the thickness of the heat conducting portion is preferably 1 μm to 500 μm.
[0248] There are no particular restrictions on the coating method using the carbon ink and the coating method using the ceramic paste, and they can be appropriately selected according to the purpose, including but not limited to spin coating, casting, micro-gravure coating, gravure coating, rod coating, roller coating, wire rod coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, dispenser coating, gravure printing, screen printing, flexographic printing, offset printing, reverse printing, inkjet and other printing methods.
[0249] In addition, when the heat conducting portion forming ink contains a monomer and a polymerization initiator, it can be cured by light or heat after coating. When the heat conducting portion is formed by an inkjet method, it is preferred to use a dispersed ink of a metal material, carbon, and a ceramic material. By dispersing the ink, the ink viscosity can be adjusted to an ink viscosity suitable for inkjet.
[0250] The viscosity of the dispersion ink is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 5 mPa·s or more and 200 mPa·s or less from the viewpoint of suitability for inkjet.
[0251] In the dispersion ink, a solvent may be used as the dispersion solvent, or a low-viscosity monomer may be used as the dispersion solvent. As the material of the dispersion solvent, the same material as the solvent in the adhesive portion forming ink may be used.
[0252] The content of the conductive material in the dispersed ink is not particularly limited and can be appropriately selected according to the purpose, but is preferably 15% by mass or more and 80% by mass or less of the total amount of the dispersed ink. If the content of the conductive material in the dispersed ink is 15% by mass or more, a thermal conductive effect can be easily obtained, and if it is 80% by mass or less, the viscosity can be reduced, and it can be suitable for inkjet printing.
[0253] <<<Other Ingredients>>>
[0254] The other components are not particularly limited and may be appropriately selected according to the purpose, and include, but are not limited to, resins, monomers, polymerization initiators, solvents, dispersants, and the like.
[0255] As the resin, the monomer, the polymerization initiator and the solvent, the same materials as those of the adhesive portion forming ink can be used, and the preferred forms are also the same, so the description is omitted. The preferred forms of the solvent and the monomer when used as the dispersion ink are also as described above.
[0256] -Dispersant-
[0257] There is no particular limitation on the dispersant, and it can be appropriately selected according to the purpose, and examples thereof include, but are not limited to, multifunctional comb-type functional polymers having ionic groups in the main chain and polyoxyalkylene chains in the side chains. The ionic groups function as adsorption groups on the surface of the powder, and the side chains impart control of the solubility of the solvent and a stereoscopic repulsion effect. As specific examples of the dispersant, alkyl mercaptans such as dodecanethiol, polyvinylpyrrolidone polymers, etc. are included but are not limited to. These can be used alone or in combination with other.
[0258] The dispersant can be suitably synthesized or a commercial product can be used. Commercial products of the dispersant include, but are not limited to, MALIALIM (registered trademark), MALIALIM SC (registered trademark), MALIALIM FA (registered trademark), ESLEAM C (registered trademark), ESLEAM MP (registered trademark), ESLEAM AD (registered trademark), ESLEAM 221P (registered trademark) (manufactured by NOF Corporation), etc.
[0259] The content of the other components in the heat transfer portion forming ink is not particularly limited and can be appropriately selected according to the purpose, but the solid content of the resin, the dispersant, the monomer cured product, etc. is preferably 5% by mass or less. Thus, the heat transfer portion can be formed in which the content of the heat transfer material in the heat transfer portion is 95% by mass or more by decomposition or gasification removal during sintering.
[0260] The heat transfer portion forming ink may be prepared as appropriate, or a commercially available ink may be used.
[0261] When the thermally conductive material contains a metal material, in addition to the method of using an ink containing the metal material, a method of reducing and precipitating a metal solution ink can also be used. Generally, silver salt inks are known, and these inks can also be used.
[0262] Examples of commercially available products of the heat transfer section forming ink include those listed in the following Table 1. These may be used alone or in combination with other products.
[0263] [Table 1]
[0264]
[0265] <Other Processes>
[0266] The other steps in the method for producing the adhesive structure are not particularly limited and may be appropriately selected according to the purpose, such as a sintering step.
[0267] 《Sintering process》
[0268] The sintering step is a step of sintering the metal nanoparticles after the heat transfer section forming step. Therefore, in the heat transfer section forming step, when the heat transfer section forming ink contains metal nanoparticles, the sintering step is preferably performed.
[0269] The sintering method is not particularly limited and can be appropriately selected from known methods, and examples thereof include methods of sintering using heat or light, etc. In this way, a heat-conducting portion having high thermal conductivity in which the metal nanoparticles are sintered can be formed.
[0270] In addition, the firing step of the heat conductive portion forming ink may also serve as a thermal curing step of at least one of the adhesive portion forming ink and the low elastic portion forming ink, for example, a step of bonding the adhesive structure to a contact object.
[0271] Next, an adhesive layer as an example of the adhesive structure will be described in detail using the drawings, but the adhesive structure of the present invention is not limited thereto.
[0272] As described above, the adhesive layer is composed of at least an adhesive portion and a low elastic portion, and may optionally further include a heat conducting portion.
[0273] [Adhesive layer example 1]
[0274] Figure 1A and Figure 1B This is an example of an embodiment of the adhesive structure of the present invention (hereinafter sometimes referred to as "adhesive layer embodiment 1"). Figure 1A : is a schematic cross-sectional view of the thickness direction of the adhesive layer 10 (a cross-sectional view in the X direction through the center of the Y axis in the plane direction; Figure 1B B-B' section). Figure 1B yes Figure 1A A schematic cross-sectional view of the adhesive layer 10 in the plane direction (a cross-sectional view in the XY direction through the center in the thickness direction; Figure 1A The adhesive layer 10 is patterned to form a plurality of adhesive portions 1 in the low elastic portion 2. In addition, the cross section of the adhesive layer 10 in the plane direction is the same pattern as the outermost layer (exposed surface, i.e., top view or bottom view) in the plane direction. Figure 1B In the example, the vertical axis is set as the Y axis and the horizontal axis is set as the X axis. Figure 1A and Figure 1B The adhesive layer 10 is formed between the heating element 30 and the substrate 20 as shown in [Configuration Example 1] to [Configuration Example 6] described later, but the present invention is not limited thereto.
[0275] [Conventional adhesive layer]
[0276] Figure 2A and Figure 2B A schematic diagram showing a conventional adhesive layer having stress relaxation properties (see Japanese Unexamined Patent Application Publication No. 2011-084743). Figure 2A is a schematic cross-sectional view of a conventional adhesive layer 100 in the thickness direction ( Figure 2B B-B' section). Figure 2B yes Figure 2A A schematic cross-sectional view of the adhesive layer 100 in the plane direction ( Figure 2A A-A' section). Figure 2A and Figure 2B The adhesive layer 100 shown is a structure in which the adhesive portion 101 is formed on the low elastic portion 102 with a phase separation island structure (phase separation island structure), and is formed roughly uniformly in the thickness direction and plane direction of the adhesive layer in order to phase separate from the layer mixed with the low elastic material and the adhesive material.
[0277] Similarly, an adhesive layer (ACRYSET (registered trademark) BP, manufactured by Nippon Shokubai Co., Ltd.) in which elastic rubber (low elasticity portion) is mixed with epoxy resin (adhesive portion) has also been proposed, but the elastic rubber is formed roughly uniformly in the thickness direction and the plane direction, and the adhesiveness and stress relaxation characteristics are poor. In particular, in a thin adhesive layer of about 1 μm to 50 μm, large-diameter rubber particles cannot be uniformly mixed, and in addition, the length of the plane direction of the low elasticity portion cannot be made to be more than 10 μm, and there is also a problem that it is difficult to obtain a stress relaxation effect. In the case of forming the above-mentioned phase separation sea island structure, it is also difficult to control the size.
[0278] In the adhesive structure of the present invention, the patterning of the adhesive portion 1 and the low elastic portion 2 can be appropriately adjusted to obtain the adhesiveness and stress relaxation properties required for the adhesive layer 10, for example, Figure 3A to Figure 3I and Figure 4A to Figure 4H As shown, various patterns such as dots, lines, rings, lattices, and radials can be provided. It is particularly preferred to form a large number of low elastic parts 2 at locations with large thermal stress (strain) and to form a large number of adhesive parts 1 on the adhesive surface. Figures 3A to 3I is a schematic diagram showing various modes of patterning in the thickness direction of an adhesive structure, Figures 4A to 4H Schematic diagrams showing various modes of patterning in the planar direction of an adhesive structure.
[0279] [Adhesive layer example 2]
[0280] Figure 3A 2 is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter, sometimes referred to as "adhesive layer embodiment 2"), in which a large number of adhesive portions 1 are formed on the contact surface of the heating element 30, which is different from the adhesive layer embodiment 1. In the case where the linear thermal expansion coefficients of the substrate 20 and the heating element 30 are different and the thermal expansion of the substrate 20 is large, by increasing the amount of the low elastic portion 2 on the substrate 20 side, the substrate 20 side is easy to expand and contract, and the stress can be effectively relieved. On the other hand, by increasing the amount of the adhesive portion 1 on the contact surface with the higher temperature heating element 30, the adhesiveness can be improved.
[0281] [Adhesive layer example 3]
[0282] Figure 3B 1 is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter sometimes referred to as "adhesive layer embodiment 3"), in which the low elastic portion 2 forms a large trapezoidal adhesive layer on the contact surface with the substrate 20, which is different from the adhesive layer embodiment 2. By changing the ratio of the adhesive portion 1 and the low elastic portion 2 in the thickness direction, the adhesiveness and stress relaxation performance can be easily adjusted.
[0283] [Adhesive layer example 4]
[0284] Figure 3C This is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter, sometimes referred to as "adhesive layer embodiment 4"), in which the amount of the low elastic portion 2 is greater in the peripheral portion in the plane direction (the region close to the exposed portion in the thickness direction), which is different from adhesive layer embodiment 3. Generally speaking, the more the peripheral portion is, the greater the deformation, so by increasing the amount of the low elastic portion in the peripheral portion, the deformation can be effectively alleviated.
[0285] [Adhesive layer example 5]
[0286] Figure 3D 1 is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter sometimes referred to as "adhesive layer embodiment 5"), in which the low elasticity portion 2 is not formed on both contact surfaces in the planar direction of the adhesive layer 10 (the exposed portion of the outermost layer in the planar direction), which is different from the adhesive layer embodiment 2. By forming the low elasticity portion 2 inside the adhesive layer 10, the adhesiveness of the contact surface and the stress relaxation characteristics inside the adhesive layer 10 can be effectively obtained.
[0287] [Adhesive layer example 6]
[0288] Figure 3E1 is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter, sometimes referred to as "adhesive layer embodiment 6"), in which the low elastic portion 2 is patterned in the film thickness direction of the adhesive layer 10, which is different from the adhesive layer embodiment 5. By also patterning the low elastic portion 2 in the thickness direction, it is possible to fine-tune the adhesiveness and stress relaxation characteristics. In addition, warping is generally generated on the adhesive layer 10 due to stress, but since the stress in the center of the thickness direction of the adhesive layer 10 tends to decrease, by increasing the amount of the adhesive portion 1 in the center of the thickness direction (i.e., reducing the amount of the low elastic portion 2), it is possible to coordinate the stress change and take into account both effective stress relaxation and adhesiveness.
[0289] [Adhesive layer example 7]
[0290] Figure 3F It is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter sometimes referred to as "adhesive layer embodiment 7"). In the thickness direction of the adhesive layer 10, the low elastic portion 2 is randomly arranged, and the low elastic portion 2 is more distributed on the two end sides of the adhesive layer 10 (the exposed portion side in the planar direction), which is different from the adhesive layer embodiment 6.
[0291] [Adhesive layer example 8]
[0292] Figure 3G It is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter sometimes referred to as "adhesive layer embodiment 8"), in which a heat conductive portion 3 continuous in the thickness direction of the adhesive layer 10 is formed between the low elastic portions 2 on the contact surface with the substrate 20, which is different from the adhesive layer embodiment 3.
[0293] [Adhesive layer example 9]
[0294] Figure 3H It is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter sometimes referred to as "adhesive layer embodiment 9"), in which a thermally conductive portion 3 continuous in the thickness direction of the adhesive layer 10 is formed between one adjacent adhesive portion 1 and another adjacent adhesive portion 1 on the contact surface with the substrate 20, which is different from the adhesive layer embodiment 3.
[0295] [Adhesive layer example 10]
[0296] Fig. 3I It is a schematic cross-sectional view in the thickness direction of another example of an embodiment of the adhesive structure of the present invention (hereinafter sometimes referred to as "adhesive layer embodiment 10"), in which the low elastic portion 2 is formed inside the adhesive layer 10 in the thickness direction, which is different from the adhesive layer embodiment 9.
[0297] In adhesive layer examples 8 to 10, the thermal conductivity of the adhesive layer 10 in the thickness direction can be improved by forming the thermal conductive part 3, thereby providing a heat dissipation effect. In addition, when the thermal conductive part 3 also serves as a conductive layer, a conductive effect can be provided.
[0298] Figure 4A This is a plan view in the planar direction showing an example of an embodiment of an adhesive structure in which the radial low-elasticity portion 2 is patterned in the planar direction. Figure 4B This is a plan view in the planar direction showing an example of an embodiment of an adhesive structure in which the low elastic portion 2 is patterned and formed in a ring shape in the planar direction. Figure 4C A plan view in the planar direction showing an example of an embodiment of an adhesive structure in which the low elastic portion 2 is patterned in a lattice shape in the planar direction. Figure 4D This is a plan view in the planar direction showing an example of an embodiment of an adhesive structure in which the low elastic portion 2 is patterned in the outer peripheral portion of the adhesive layer where stress is likely to concentrate in the planar direction. Figure 4E It means in Figure 4D A plan view in the planar direction of an example of an embodiment of an adhesive structure in which a cross-lattice-shaped low elastic portion 2 is further patterned in the planar direction. In addition, Figure 4A , Figure 4B , Figure 4C , Figure 4D and Figure 4E The patterning formation in the process can have the same pattern on the exposed surface (top view) and the cross section in the plane direction, or can have different patterns on the exposed surface and the cross section in the plane direction.
[0299] Figure 4F , 4G 4H and 4H are plan views showing an example of an embodiment of an adhesive structure used when forming a wire bond on the surface of a heat generating element (eg, a chip). Figure 4F and Figure 4G In the figure, a low elastic portion 2 is formed at the upper end and the lower end, and a wire bonding contact portion 4 is formed by penetrating the low elastic portion 2, thereby effectively alleviating the deformation caused by the formation of wire bonding. That is, the adhesive structure can improve the stress relaxation performance by patterning the elastic adjustment of the part that is prone to deformation (for example, the contact part with the wiring part such as wire bonding, flip chip, etc.). In addition, by using the ink for forming the low elastic portion, pattern coating can be performed with good filling properties, and the generation of bubbles and gaps that become the starting point of peeling of the adhesive structure can be suppressed. In this case, it is effective to coat by inkjet method. Any pattern can be formed by inkjet method, and a thin film and excellent uniformity adhesive structure can be formed at the same time. In addition, pattern coating can be performed avoiding wiring parts such as wire bonding and flip chip.
[0300] Figure 4H This is an embodiment in which the adhesive layer 10 is patterned for the purpose of achieving the same effect, and the adhesive layer 10 is not formed around the wire bonding contact portion 4 .
[0301] Figure 4F , Figure 4G and Figure 4H As described later Figure 7B Example 3 and Figure 8B In the structure in which an adhesive layer is formed between heating elements (semiconductor: chips) as in the configuration example 4, it is effective when wire bonding is formed on the heating element. Figure 4F , Figure 4G and Figure 4H The patterning in the film may have the same pattern on the exposed surface and in the thickness direction, or may have different patterns on the exposed surface and in the thickness direction.
[0302] (Adhesive layer for transfer)
[0303] The transfer pressure-sensitive adhesive layer of the present invention has the pressure-sensitive adhesive structure of the present invention in a layered form on a temporary support.
[0304] The details of the adhesive structure of the present invention are the same as those described in the above-mentioned "Adhesive structure and method for producing an adhesive structure", and will not be described again.
[0305] <Temporary Support>
[0306] The temporary support is not particularly limited as long as the adhesive structure can be manufactured on its surface and has no influence on the adhesive portion, the low elastic portion, the thermal conductive portion, and any other optional components patterned in the adhesive structure, and a known release sheet can be used.
[0307] The release sheet is not particularly limited and can be appropriately selected according to the purpose, for example, kraft paper, glassine paper, high-grade paper, etc.; resin films such as polyethylene, polypropylene (biaxially oriented polypropylene (OPP), uniaxially oriented polypropylene (CPP)), polyethylene terephthalate (PET), etc.; laminated paper formed by laminating the above paper and resin films; a material in which a sealant treatment is applied to one or both sides of the above paper with clay or polyvinyl alcohol, etc. and a release treatment such as silicone resin is applied, etc. These can be used alone or in combination with others.
[0308] The method for forming the layered adhesive structure on a temporary support is not particularly limited, and the adhesive structure can be formed in the same manner as in the method for producing the adhesive structure except that the contact object is replaced by the support.
[0309] The advantage of the transfer adhesive layer is that the adhesive structure is easy to store and transport and has excellent operability. Even if the adhesive structure cannot be directly formed on the contact object, the adhesive structure can be easily formed on the contact object by sticking the transfer adhesive layer on the contact object and peeling off the support.
[0310] (Electronic component and method for manufacturing electronic component)
[0311] The electronic component of the present invention has at least the adhesive structure of the present invention and may further have other components as necessary. The details of the adhesive structure of the present invention are the same as those described in the above "Adhesive structure and method for producing adhesive structure" and will not be described in detail.
[0312] The method for producing an electronic component of the present invention includes fixing components using the adhesive structure of the present invention and may further include other steps as necessary.
[0313] The method for fixing the member using the pressure-sensitive adhesive structure is not particularly limited and may be appropriately selected depending on the configuration of the pressure-sensitive adhesive structure. Examples thereof include photocuring and thermal curing.
[0314] <First Element and Second Element>
[0315] The electronic component preferably includes a first component and a second component fixed by the adhesive structure.
[0316] The difference in linear thermal expansion coefficient between the first element and the second element is not particularly limited and can be appropriately selected according to the purpose, but is preferably less than 20ppm / K, more preferably less than 10ppm / K. If the difference in linear thermal expansion coefficient is less than 20ppm / K, the warping of the adhesive structure is small. The smaller the difference in linear thermal expansion coefficient between the first element and the second element, the better, and its lower limit is not particularly limited. Since the electronic component of the present invention has the adhesive structure of the present invention, even if the difference in linear thermal expansion coefficient is high, the adhesion and stress relaxation properties are excellent, and poor adhesion and poor connection can be suppressed. In particular, the low elasticity portion in the adhesive structure can suppress the deformation caused by the difference in linear thermal expansion coefficient between the first element and the second element.
[0317] The difference in linear thermal expansion coefficient between the first element and the second element may be measured by a thermomechanical analyzer (eg, TMA (Themomechanical Analysis)).
[0318] There is no particular limitation on the first element and the second element, and they can be appropriately selected according to the type of target electronic component. For example, the first element can be a heating element and the second element can be a substrate, the first element can be a cooling element and the second element can be a substrate, etc.
[0319] The heating element is not particularly limited and can be appropriately selected according to the type of target electronic component, and examples thereof include semiconductors (chips), semiconductor packages, batteries, LEDs, capacitors, resistors, diodes, etc. Among them, as the heating element, preferably, a semiconductor (IC chip) is required to have heat-resistant reliability for bonding and connection of mounting circuits due to temperature rise, as the high integration and high speed in recent years have been accompanied.
[0320] In the electronic component, the adhesive structure is preferably at least one of a chip bonding layer, a heat dissipation layer, and an anti-corrosion agent. Since the adhesive structure has the adhesive portion, it is preferably used as a chip bonding layer. In addition, when the adhesive structure has the heat conduction portion, it is also suitable for playing a role as a heat dissipation layer.
[0321] Furthermore, the electronic component may have an intermediate layer such as a surface treatment layer between the adhesive structure and the first component or the second component.
[0322] The surface treatment layer is formed as a layer for adjusting the wettability or surface energy of the adhesive structure formation surface, and is formed as a resin film having a hydrophilic group or a hydrophobic group on its surface.
[0323] There is no particular limitation on the material of the surface treatment layer, and it can be appropriately selected according to the purpose. For example, materials having carboxyl groups, amino groups, ketone groups, OH groups, fluorine groups, silanol groups, etc. in the resin structure can be used. In addition, inorganic particles such as ceramics, metals, and carbon can also be mixed. These can use the same substances as those contained in the ink for forming the thermal conductive portion.
[0324] The thickness of the surface treatment layer is not particularly limited and may be appropriately selected depending on the intended purpose, but is preferably 0.5 μm to 10 μm.
[0325] There is no particular limitation on the method for forming the surface treatment layer, and it can be appropriately selected according to the purpose. For example, it can be formed by coating a mixture of a resin material or an inorganic material mixed with an organic monomer material having at least a reactive group and an initiator, and then subjecting the mixture to curing treatment such as UV irradiation, heat treatment, and dehydration treatment.
[0326] The coating method is not particularly limited and can be appropriately selected according to the purpose. For example, various printing methods such as spin coating, casting, micro-gravure coating, gravure coating, rod coating, roller coating, wire rod coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, dispenser coating, gravure printing, screen printing, flexographic printing, offset printing, reverse printing, and inkjet printing can be used.
[0327] The electronic components may also be formed with a resist using commercially available photocurable inks, thermosetting inks, etc. Commercially available products of the resist inks include, for example, PSR-4000G24K / Ca-40G24, PSR-4000BL0 1 / Ca-40G24, PSR-4000GEC50K 1 / Ca-40G50, PSR-4000EG23 / Ca-40G23K, PSR-4000EG30 / Ca-40G23K, IJSR4000, IJSR9000 (all manufactured by Sun Ink Co., Ltd.), PSR-310, PSR-400B, PSR-500B, PR1205, PR1243, PR1258 (all manufactured by Huying Chemical Industries, Ltd.), etc.
[0328] Next, the use of the adhesive structure in the electronic component will be described in detail with reference to the drawings, but the use of the electronic component and the adhesive structure of the present invention is not limited thereto.
[0329] [Configuration Example 1]
[0330] Figure 5 1 is a schematic cross-sectional view showing an example of the configuration of an electronic component using the adhesive structure of the present invention (hereinafter, sometimes referred to as "Configuration Example 1"). Figure 5 In the embodiment, the heating element 30 and the substrate 20 are bonded to the adhesive layer 10 which is the adhesive structure of the present invention.
[0331] Specific examples of the electronic component of the heating element 30 include a semiconductor (chip), a semiconductor package, a battery, an LED, a capacitor, a resistor, a diode, and the like.
[0332] The adhesive layer 10 relieves stress caused by the difference in linear thermal expansion coefficient between the heating element 30 and the substrate 20 and maintains adhesion even when the temperature changes.
[0333] [Configuration Example 2]
[0334] Figure 6 It is a schematic cross-sectional view showing another example of the configuration of an electronic component using the adhesive structure of the present invention (hereinafter, sometimes referred to as “Configuration Example 2”).
[0335] Figure 6 In the configuration example 1, the substrate 20 is replaced with a cooling element 40 bonded thereto, and the configuration example 1 is the same as the configuration example 1 except for this.
[0336] The cooling element 40 is a component that cools the heat of the heating element 30 by air cooling, liquid cooling, phase change cooling, thermoelectric cooling, or the like.
[0337] Specific examples of the cooling element 40 include a heat sink, a heat pipe, a microchannel, a Peltier element, a heat sink, a radiator, and the like.
[0338] [Configuration Example 3]
[0339] Fig. 7A and Figure 7B It is a schematic cross-sectional view showing another example of the configuration of an electronic component using the adhesive structure of the present invention (hereinafter, sometimes referred to as “Configuration Example 3”).
[0340] Fig. 7A and 7B The difference from Configuration Example 1 is that another heating element 30 - 2 is bonded to the heating element 30 - 1 via an adhesive layer 10 . Fig. 7A and 7B The configuration is effective in the case of stacking the heating element 30 - 1 and the heating element 30 - 2 and in the case of reducing the temperature difference between the heating element 30 - 1 and the heating element 30 - 2 to make it uniform. Figure 7B This shows an example in which the heating element is a semiconductor (chip) and has a wiring portion 60 on the heating element 30 - 1 , and specifically, wire bonding is performed from the upper surface of the heating element 30 - 1 .
[0341] [Configuration Example 4]
[0342] Fig. 8A and Figure 8B It is a schematic cross-sectional view showing another example of the configuration of an electronic component using the adhesive structure of the present invention (hereinafter, sometimes referred to as “Configuration Example 4”).
[0343] Fig. 8A and 8B The difference from the structural form example 1 is that another heating element 30 - 2 is bonded to the heating element 30 - 1 through another adhesive layer 10 - 2 , and the heating element 30 - 1 and the substrate 20 are bonded through the adhesive layer 10 - 1 . Figure 8BIn the embodiment, the heating element has a wiring portion 60 on the heating element 30-1 as a semiconductor (chip). Specifically, it is an example of wire bonding from the upper surface of the heating element 30-1. The bonding portion and the low elastic portion in the bonding layer 10-1 and the bonding layer 10-2, as well as the pattern of the heat conducting portion as required, and the thickness of the bonding layer 10-1 and the bonding layer 10-2 can be appropriately selected independently. That is, the bonding portion, the low elastic portion and the heat conducting portion in the bonding layer 10-1 and the bonding layer 10-2 can be the same pattern or different patterns. In addition, the thickness of the bonding layer 10-1 and the bonding layer 10-2 can be the same or different. Among them, from the viewpoint of bonding force and stress relaxation characteristics, it is preferred that the patterns of the bonding portion, the low elastic portion and the heat conducting portion in the bonding layer 10-1 and the bonding layer 10-2 are different patterns, and the thickness of the bonding layer 10-1 and the bonding layer 10-2 selects different thicknesses.
[0344] [Configuration Example 5]
[0345] Fig. 9A and Fig. 9B It is a schematic cross-sectional view showing another example of the configuration of an electronic component using the adhesive structure of the present invention (hereinafter, sometimes referred to as “Configuration Example 5”).
[0346] Fig. 9A The difference from Configuration Example 1 is that an intermediate layer 50 is formed between the substrate 20 and the adhesive layer 10 . Fig. 9B The difference from Configuration Example 1 is that an intermediate layer 50 is formed between the heating element 30 and the adhesive layer 10 .
[0347] An intermediate layer 50 may be formed at least between the adhesive layer 10 and the substrate 20, and between the adhesive layer 10 and the heating element 30. The intermediate layer 50 is not particularly limited and may be appropriately selected according to the purpose, for example, a heat dissipation portion for diffusing heat in a planar direction and a surface treatment portion for improving adhesion.
[0348] [Configuration Example 6]
[0349] Fig.10 It is a schematic cross-sectional view showing another example of the configuration of an electronic component using the adhesive structure of the present invention (hereinafter, sometimes referred to as “Configuration Example 6”). Fig.10 The difference from Configuration Example 1 is that an adhesive layer 10 is formed between electrodes 501 and 502. Configuration Example 6 is effective when the electrodes are insulated from each other or when the electrodes are electrically connected to each other.
[0350] As the material of the electrode 501 and the electrode 502, general electrode materials can be used. As specific examples of the material of the electrode, silver (Ag), copper (Cu), gold (Au), aluminum (Al), nickel (Ni), tin (Sn), platinum (Pb), carbon materials, etc. can be cited. These can be used alone or in combination with others. The electrodes can be divided and formed into wiring patterns.
[0351] The method for manufacturing the electronic component is not particularly limited as long as it includes the step of fixing a component using the adhesive structure, and can be appropriately selected according to the purpose. The component can be fixed using the transfer adhesive layer of the present invention, or the adhesive structure can be directly formed on the component that is the contact object.
[0352] In the electronic component, when the adhesive structure is a resist, the following method is preferred: it includes a first resist layer forming step, on a substrate at a position corresponding to a first area of an edge portion of the obtained resist pattern, an adhesive portion forming ink for forming an adhesive portion capable of adhering to a contact object is discharged from a nozzle, and the adhesive portion is set to form a first resist layer; a second resist layer forming step, on the substrate at a position corresponding to a second area different from the first area, a low elastic portion forming ink for forming a low elastic portion having an elastic modulus smaller than that of the adhesive portion is discharged from a nozzle, and the low elastic portion is set in a patterned manner to form a second resist layer; and a resist pattern forming step, the first resist layer and the second resist layer are cured to form a resist pattern. In the first resist layer forming process and the second resist layer forming process, it is preferred that the adhesive portion forming ink and the low elastic portion forming ink are simultaneously arranged on the substrate to form a resist pattern in which the first area portion of the resist pattern formed by the adhesive portion forming ink and the second area portion of the resist pattern formed by the low elastic portion forming ink are connected.
[0353] The ejection of the adhesive portion forming ink, the ejection of the low elastic portion forming ink, the patterning of the low elastic portion forming ink, etc. when forming the resist can be carried out by the same method as the method for producing the adhesive structure of the present invention.
[0354] [Example]
[0355] Hereinafter, the present invention will be specifically described by way of preparation examples, embodiments and comparative examples, and the present invention includes but is not limited to these preparation examples and embodiments. In addition, in the following preparation examples, embodiments and comparative examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0356] As materials for the adhesive portion forming ink and the low elastic portion forming ink in the following preparation examples, materials shown in the following Table 2 were prepared. In addition, in the following Table 2, the viscosity of each material is also shown.
[0357] [Table 2]
[0358]
[0359] [Chemical formula 4]
[0360]
[0361] <Viscosity Measurement Method>
[0362] In the following preparation examples, the viscosity of each ink was measured by a cone-plate rotational viscometer (VISCOMETER TVE-22L, manufactured by Toki Sangyo Co., Ltd.) using a conical rotor (1°34'×R24) at a rotation speed of 10 rpm and a constant temperature circulating water temperature of 25° C. The temperature of the circulating water was adjusted using a circulating thermostatic bath (e.g., VISCOMATE VM-150III, manufactured by Toki Sangyo Co., Ltd.).
[0363] (Preparation Example 1-1: Preparation of Adhesive Section Forming Ink A-1)
[0364] 60 parts of glycidyl ether type monofunctional epoxy monomer OCR-EP (manufactured by Yokkaichi Synthetic Co., Ltd.), 20 parts of glycidyl ether type tetrafunctional epoxy monomer PETG (manufactured by Showa Denko K.K.), 20 parts of glycidyl amine type tetrafunctional epoxy monomer TETRAD-X (manufactured by Mitsubishi Gas Chemical Co., Ltd.) and 1 part of thermal polymerization initiator (SAN-AID SI-150L) were mixed to prepare a thermal curing [adhesive portion forming ink A-1]. The viscosity of [adhesive portion forming ink A-1] at 25° C. was 22.9 mPa·s, which is a viscosity suitable for inkjet printing.
[0365] (Preparation Example 1-2: Preparation of Adhesive Section Forming Ink A-2)
[0366] 100 parts of an alicyclic epoxy monomer (EPOCALIC THI-DE, manufactured by ENEOS) and 1 part of a thermal polymerization initiator (SAN-AID SI-150L) were mixed to prepare a heat-curable [adhesive portion forming ink A-2]. The viscosity of [adhesive portion forming ink A-2] at 25° C. was 19.3 mPa·s, which is a viscosity suitable for inkjet printing.
[0367] (Preparation Example 1-3: Preparation of Adhesive Section Forming Ink A-3)
[0368] 36 parts of an alicyclic epoxy monomer (EPOCALIC THI-DE, manufactured by ENEOS), 12 parts of a glycidylamine-type tetrafunctional epoxy monomer TETRAD-X (manufactured by Mitsubishi Gas Chemical Co., Ltd.), 32 parts of an oxetane monomer (ARON 0XETANEOXT-221, manufactured by Toagosei Co., Ltd.), 19 parts of an oxetane acrylic monomer (OXE-10, manufactured by Osaka Organic Chemical Industry Co., Ltd.), 2 parts of a multifunctional dipentaerythritol polyacrylic monomer (A-DPH, manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), 0.1 parts of a photopolymerization initiator (Irgacure TPO, manufactured by IGM Resins BV) and 0.8 parts of a thermal polymerization initiator (SAN-AIDSI-150L, manufactured by Sanshin Chemical Industry Co., Ltd.) were mixed to prepare [Ink A-3 for forming an adhesive portion] that is cured by light and heat. The viscosity of [Adhesive portion forming ink A-3] at 25° C. was 32.0 mPa·s, which was a viscosity suitable for inkjet printing.
[0369] (Preparation Example 2-1: Preparation of Low Elasticity Section Forming Ink B-2)
[0370] 50 parts of alicyclic epoxy monomer (CEL8010P, manufactured by Daicel), 50 parts of oxetane monomer (ARONOXETANE 0XT-212, manufactured by Toagosei Co., Ltd.) and 1.0 part of thermal polymerization initiator (SAN-AID SI-150L, manufactured by Sanshin Chemical Co., Ltd.) were mixed and thermally cured to prepare [low elastic portion forming ink B-2]. [Low elastic portion forming ink B-2] had a viscosity of 28.1 mPa·s at 25° C., which was a viscosity suitable for inkjet printing.
[0371] <Measurement of Indentation Elastic Modulus of Cured Film>
[0372] The indentation elastic modulus of the cured products of [Adhesive portion forming ink A-1] to [Adhesive portion forming ink A-3] obtained in Preparation Examples 1-1 to 1-3, SUN-013 (manufactured by Sekisui Chemical Co., Ltd.) prepared as low elastic portion forming ink B-1, and [Low elastic portion forming ink B-2] obtained in Preparation Example 2-1 was measured by the following method.
[0373] After inkjet printing on a glass surface with a thickness of 10 mm, the [adhesive portion forming ink A-1] to [adhesive portion forming ink A-3] obtained in Preparation Examples 1-1 to 1-3, SUN-013 (manufactured by Sekisui Chemical Co., Ltd.) prepared as the low elastic portion forming ink B-1, and the [low elastic portion forming ink B-2] obtained in Preparation Example 2-1 were heated at 100° C. for 2 hours, and further heat-cured at 200° C. for 1 hour to prepare a cured film with a thickness of 15 μm. In addition, for light and heat curable inks, Honle LEDcube100 (manufactured by Honle uv technology) was used before heat curing, and the heat curing was performed after pre-light curing with UV LED (365 nm). As an inkjet device, a single nozzle ultrafine inkjet device (manufactured by CLUSTER SPUTTER) was used, and a device with a nozzle aperture of 25 μm was used.
[0374] The indentation modulus of each cured film prepared by the above method was measured using a microhardness tester (FISCHERSCOPE (registered trademark) HM2000, manufactured by Fischer Instruments) under the following measurement conditions. The measurement results of the indentation modulus of each ink cured film are shown in the following Tables 3-1 and 3-2.
[0375] [Measurement conditions]
[0376] Indenter: Vickers Indenter
[0377] Maximum load: 10mN
[0378] Maximum indentation depth: 1μm
[0379] Loading (unloading) time: 40 seconds
[0380] [Table 3-1]
[0381]
[0382] [Table 3-2]
[0383]
[0384] (Example 1)
[0385] In Example 1, the Fig.11A and Fig. 11B The layered adhesive structure shown.
[0386] In order to evaluate the adhesive force of the adhesive structure, a printed wiring board (PWB) substrate 300 and a silicon substrate 200 were bonded together using the adhesive structure 10 as a bonding sample. The low elasticity portion 2 and the adhesive portion 1 of the adhesive structure 10 were formed by inkjet printing. The inkjet device used was an inkjet device (Stage JET, manufactured by Tritec) equipped with MH 5420 (manufactured by Ricoh Co., Ltd.) as a nozzle.
[0387] The specific method is as follows.
[0388] <Preparation of Adhesive Samples from Layered Adhesive Structures>
[0389] -Substrate Preparation-
[0390] A square printed wiring board (PWB) substrate (a substrate obtained by coating and curing a glass epoxy RF-4 surface with an anti-corrosion agent) having a length of 10 mm, a width of 10 mm, and a thickness of 1.6 mm was prepared. The anti-corrosion agent used was PSR-4000SP19A / CA-40SP19A (manufactured by Sunholding Co., Ltd.). The linear thermal expansion coefficient of the PWB substrate was 15.7 ppm / K, and the linear thermal expansion coefficient of silicon was 3.34 ppm / K.
[0391] -design-
[0392] like Fig. 11B As shown in FIG. 1 , a square adhesive structure forming area with a side length of 5 mm is designed at the center of the plane direction of the PWB substrate. At this time, the center of the adhesive structure forming area is made to be the same as the center of the PWB substrate. A low elastic portion forming area is designed with a width of 0.35 mm around the square adhesive structure forming area with a side length of 4.3 mm.
[0393] -Formation of low elasticity portion-
[0394] As the ink for forming the low elastic part, [Ink B-1 for forming the low elastic part] in Table 3-2 of the material in Table 2 was used, and based on the design, the low elastic part forming area on the PWB substrate was inkjet printed. Then, the ejected droplets were pre-photocured with UV LED (365nm) using Honle LEDcube100 (manufactured by Honle uv technology) to form a low elastic part with an average thickness of 15μm and a width of 0.5mm.
[0395] -Formation of Adhesive Section-
[0396] Next, as the ink for forming the adhesive portion, [Ink A-1 for forming the adhesive portion] of Table 3-1 of the material of Table 2 was used, and based on the design, inkjet printing was performed on the adhesive portion forming area of the square with a side length of 4.3 mm inside the low elastic portion formed on the PWB substrate to form the adhesive portion. At this time, the droplet amount of [Ink A-1 for forming the adhesive portion] was controlled so that the average thickness was 15 μm. Thus, a adhesive portion having a thickness of 1.5 μm was formed on the PWB substrate 300. Fig.11A and 11B The layered bonded structure 10 includes a bonding portion 1 and a low elastic portion 2.
[0397] Then, if Fig.11A and Fig. 11B As shown, a square silicon substrate 200 with a length of 5 mm, a width of 5 mm and a thickness of 0.4 mm is bonded to the adhesive structure 10 on the opposite side of the adhesive structure 10 which is in contact with the PWB substrate 300, and then heated at 100°C for 2 hours and then heat-cured at 200°C for 1 hour, thereby preparing a sample of the adhesive structure of Example 1 in which the PWB substrate 300 and the silicon substrate 200 are bonded using the adhesive structure 10.
[0398] The average film thickness of the low elasticity portion and the adhesive portion is an average value of three arbitrary locations of the low elasticity portion or the adhesive portion measured with a probe meter (Alpha-Step D-500, manufactured by KLA-Tenchore Corporation).
[0399] (Example 2)
[0400] In addition to changing the plane pattern of the low elastic part to Figure 4E Except for the pattern shown, the adhesive sample of the layered adhesive structure of Example 2 was produced in the same manner as in Example 1. Figure 4E In the pattern shown, Fig. 11B The pattern of the adhesive portion shown is divided into nine parts in the planar direction by the low elastic portion having a width of 0.15 mm which is continuous in the thickness direction of the adhesive structure.
[0401] (Example 3)
[0402] In Example 1, the layered adhesive structure of Example 3 was prepared in the same manner as in Example 1, except that the [low elastic portion forming ink B-1] was changed to the [low elastic portion forming ink B-2] and ejected. In addition, since the [low elastic portion forming ink B-2] was a thermosetting ink, the photocuring treatment was not performed.
[0403] (Example 4)
[0404] A layered adhesive structure of Example 4 was prepared in the same manner as in Example 3 except that the [adhesive portion forming ink A-1] in Example 3 was changed to the [adhesive portion forming ink A-2].
[0405] (Example 5)
[0406] In Example 5, the preparation Fig. 12A and Fig. 12B The layered adhesive structure shown.
[0407] In order to evaluate the adhesive force of the layered adhesive structure, a PWB substrate 300 and a silicon substrate 200 were bonded together using the adhesive structure as a bonding sample. The PWB substrate, the resist, and the silicon substrate used were the same materials as in Example 1.
[0408] The low elasticity portion 2 and the adhesive portion 1 of the adhesive structure 10 were formed by inkjet printing. The inkjet device was the same as that in Example 1.
[0409] The specific method is as follows.
[0410] <Preparation of Adhesive Sample of Layered Adhesive Structure>
[0411] -design-
[0412] like Fig. 12B As shown in FIG. 1 , a square adhesive structure forming area with a side length of 5 mm is designed at the center of the plane direction of the PWB substrate. At this time, the center of the adhesive structure forming area is made to be the same as the center of the PWB substrate. A low elastic portion forming area with a width of 0.2 mm is designed around the adhesive structure forming area.
[0413] In Example 5, a heat transfer portion forming region is designed in the adhesive structure forming region. Specifically, the heat transfer portion forming region of a perfect circle with a radius of 2 mm is designed to be 4 in length and 4 in width, a total of 16, and the center-to-center distance of the heat transfer portion forming region is 10 mm. In addition, the shortest distance between the low elastic portion forming region and the outer periphery of the heat transfer portion forming region is designed to be 8.8 mm.
[0414] -Formation of low elasticity portion-
[0415] As the low elastic portion forming ink, [low elastic portion forming ink B-1] in Table 3-2 of the material in Table 2 was used, and inkjet printing was performed in the low elastic portion forming region on the PWB substrate based on the design.
[0416] Then, the ejected droplets were pre-photocured with UV LED (365 nm) using Honle LEDcube100 (manufactured by Honle uv technology), thereby forming a low elastic portion having an average thickness of 15 μm and a width of 0.2 mm.
[0417] -Formation of Adhesive Section-
[0418] Next, as the ink for forming the adhesive portion, [Ink A-3 for forming the adhesive portion] of Table 3-1 of the material of Table 2 was used, and based on the design, inkjet printing was performed on the area (the adhesive portion forming area) other than the area for forming the heat conductive portion inside the low elastic portion formed on the PWB substrate. In addition, Honle LEDcube100 (manufactured by Honle uv technology) was used to pre-light cure the ejected droplets with UV LED (365nm). At this time, the droplet amount of [Ink A-3 for forming the adhesive portion] was controlled so that the average thickness was 15μm.
[0419] -Formation of heat transfer part-
[0420] Next, Ag nanoparticle ink (SMART INK Smart Jet 1 (S-CS01520), manufactured by Genes INK) was used as the ink for forming the heat transfer portion, and inkjet printing was performed on the heat transfer portion forming region based on the above design. In addition, the solvent of the deposited Ag nanoparticle ink was removed by heating the PWB substrate at 100° C. during inkjet printing of the ink for forming the heat transfer portion.
[0421] Therefore, the following is formed on the PWB substrate 300: Fig. 12A and 12B The layered adhesive structure 10 of the adhesive portion 1 , the low elastic portion 2 and the heat conductive portion 3 is shown.
[0422] Next, a square silicon substrate 200 having a length of 5 mm, a width of 5 mm, and a thickness of 0.4 mm was bonded to the surface of the adhesive structure 10 opposite to the surface in contact with the PWB substrate 300 of the adhesive structure 10, and then heated at 100° C. for 2 hours and heat-cured at 200° C. for 1 hour, thereby preparing a Fig. 12A and 12B The sample of the structure shown is an adhesive structure 10 having a heat conducting portion 3 of Example 5 in which a PWB substrate 300 and a silicon substrate 200 are bonded together via the adhesive structure 10 .
[0423] (Comparative Example 1)
[0424] In Example 1, a bonding sample of the layered adhesive structure of Comparative Example 1 was prepared in the same manner as in Example 1 except that the design was changed so that the low elastic portion was not formed.
[0425] -design-
[0426] A square adhesive structure forming region with a side length of 5 mm was designed at the center of the plane direction of the PWB substrate. At this time, the center of the adhesive structure forming region was made to coincide with the center of the PWB substrate.
[0427] (Comparative Example 2)
[0428] A bonding sample of the layered adhesive structure of Comparative Example 2 in which the low elastic portion was not formed was prepared in the same manner as in Comparative Example 1 except that the [adhesive portion forming ink A-1] in Comparative Example 1 was changed to the [adhesive portion forming ink A-2].
[0429] (Comparative Example 3)
[0430] A bonding sample of a layered adhesive structure of Comparative Example 3 in which a low elastic portion was not formed was prepared in the same manner as in Comparative Example 1 except that the [adhesive portion forming ink A-1] in Comparative Example 1 was changed to the [low elastic portion forming ink B-1].
[0431] (Comparative Example 4)
[0432] A bonding sample of a layered adhesive structure of Comparative Example 4 in which a low elastic portion is not formed was prepared in the same manner as in Comparative Example 1, except that the [adhesive portion forming ink A-1] in Comparative Example 1 was changed to a mixed ink of [adhesive portion forming ink A-2] and [low elastic portion forming ink B-2] (A-2:B-2=74:26, mass ratio).
[0433] <Determination of chip shear strength>
[0434] As an evaluation of the adhesive strength in a heated state of the samples of Examples 1 to 5 and Comparative Examples 1 to 4, a shear strength evaluation (die shear strength evaluation) at 260° C. was performed by the following method.
[0435] The samples of Examples 1 to 5 and Comparative Examples 1 to 4 were heated to 260° C. and evaluated for shear adhesion (die shear strength) using an adhesion tester (Dage 4000, manufactured by Nordson). The measurement conditions were in accordance with JEITA Standard ED-4703K-111. The results are shown in Table 4 below.
[0436] [Table 4]
[0437]
[0438] From the results in Table 4, it was confirmed that Examples 1 to 5 had an adhesive force with good die shear strength. In addition, it was confirmed that the die shear strength was greater than that of the comparative example.
[0439] In Table 4, the ratio of the elastic modulus of the low elastic portion to the elastic modulus of the adhesive portion (elastic modulus ratio) was calculated by the following formula (1), and the volume ratio of the low elastic portion in the adhesive structure (low elastic portion content) was calculated by the following formula (2):
[0440] Elastic modulus ratio (%) = elastic modulus of low elastic part / elastic modulus of bonding part × 100 ... formula (1)
[0441] Low elastic part content (volume %) = volume of low elastic part / volume of adhesive structure as a whole × 100 ... Formula (2)
[0442] (Test Example 1: Evaluation of Characteristics of Heat Conducting Part)
[0443] A glass substrate having a length of 40 mm, a width of 40 mm, and a thickness of 1 mm was prepared, and a sample for evaluating the characteristics of the heat transfer portion was produced as follows.
[0444] -design-
[0445] A square heat transfer portion forming region with a side length of 15 mm was designed at the center of the plane direction of the glass substrate. At this time, the center of the heat transfer portion forming region was made to coincide with the center of the glass substrate.
[0446] -Formation of heat transfer part-
[0447] As the ink for forming the heat conducting portion, Ag nanoparticle ink (SMART INK Smart Jet 1 (S-CS01520), manufactured by Genes INK) was used, and inkjet printing was performed on the heat conducting portion forming region on the glass substrate based on the above design. In addition, the heat conducting portion forming ink was heated at 100° C. during inkjet coating to remove the solvent of the deposited Ag nanoparticle ink. Then, the ink was heated at 100° C. for 2 hours and then heat cured at 200° C. for 1 hour.
[0448] Thus, a heat transfer portion having a square shape of 15 mm on a side and an average thickness of 15 μm was formed on the glass substrate.
[0449] <Measurement of Volume Resistivity>
[0450] The resistance value of the produced sample was measured using a four-terminal resistance measuring machine (Loresta-GP, manufactured by Mitsubishi Chemical Analytech Co., Ltd.).
[0451] As a result, the volume resistivity of the sample was 1.0×10-5 Ω·cm.
[0452] <SEM Observation>
[0453] The prepared sample was observed using a scanning electron microscope (SEM) (NVision40 (Carl ZEISS), manufactured by SII Corporation).
[0454] The results of the SEM observation are shown in Fig.13 . According to Fig.13 , it was confirmed that the nanoparticles were bound to each other, i.e., sintered.
[0455] <Measurement of Film Thickness and Surface Roughness>
[0456] The film thickness and surface roughness of the fabricated sample were measured using a probe profilometer (Alpha-step D-500, manufactured by KLA-Tenchore Corporation).
[0457] As a result, the average thickness was 15 μm and the surface roughness was 30 nm or less.
[0458] Examples of various aspects of this embodiment include, but are not limited to, the following:
[0459] <1>
[0460] An adhesive structure, comprising:
[0461] An adhesive portion bonded to a contact object; and
[0462] A low-elasticity portion having a lower elastic modulus than that of the adhesive portion,
[0463] wherein at least one of the adhesive portion and the low-elasticity portion has a pattern shape.
[0464] <2>
[0465] The adhesive structure according to <1>, wherein the adhesive structure is a layered adhesive structure.
[0466] <3>
[0467] The adhesive structure according to <1> or <2>, wherein the shapes and sizes of a part of the adhesive portion and a part of the low-elasticity portion exposed on one surface are different from the shapes and sizes of another part of the adhesive portion and another part of the low-elasticity portion exposed on the other surface.
[0468] <4>
[0469] according to <1> ~ <3> The adhesive structure described in any one of the above, wherein at least one of the adhesive portion and the low elastic portion has a size of 10 μm or more in a planar direction of the adhesive structure.
[0470] <5>
[0471] according to <1> ~ <4> The adhesive structure described in any one of the preceding claims, wherein the volume ratio of the low elastic part to the adhesive structure is 5% to 90%.
[0472] <6>
[0473] according to <1> ~ <5> The adhesive structure described in any one of the preceding claims, wherein the elastic modulus of the low elastic portion is 70% or less of the elastic modulus of the adhesive portion.
[0474] <7>
[0475] according to <1> ~ <6> The adhesive structure described in any one of the preceding claims, wherein the elastic modulus of the low elastic portion is 3000 MPa or less.
[0476] <8>
[0477] according to <1> ~ <7> The adhesive structure described in any one of the above aspects further includes a heat conductive portion that is continuous in the thickness direction.
[0478] <9>
[0479] according to <1> ~ <8> The adhesive structure described in any one of the above, wherein at least one of the adhesive portion and the low elastic portion contains a photocurable resin.
[0480] <10>
[0481] An adhesive layer for transfer printing, comprising:
[0482] Temporary supports; and
[0483] according to <1> ~ <9> The adhesive structure described in any one of the above is a layered adhesive structure on the temporary support.
[0484] <11>
[0485] An electronic component comprising <1> ~ <9> The adhesive structure described in any one of the above.
[0486] <12>
[0487] according to <11> The electronic component further comprises:
[0488] a first element; and
[0489] A second element is fixed to the first element by the adhesive structure.
[0490] <13>
[0491] according to <12> The electronic component, wherein the difference in linear thermal expansion coefficient between the first component and the second component is 0 ppm / K to 20 ppm / K.
[0492] <14>
[0493] according to <12> or <13> The electronic component described above, wherein the low elastic portion in the adhesive structure prevents deformation caused by a difference in linear thermal expansion coefficient between the first element and the second element.
[0494] <15>
[0495] according to <12> ~ <14> The electronic component described in any one of the preceding claims, wherein the first component is a heating component or a cooling component, and the second component is a substrate.
[0496] <16>
[0497] according to <12> ~ <15> The electronic component described in any one of the preceding claims, wherein the first component is a semiconductor.
[0498] <17>
[0499] according to <11> ~ <16> The electronic component described in any one of the preceding claims, wherein the adhesive structure is at least one of a die bonding layer, a heat dissipation layer, and a resist.
[0500] <18>
[0501] A method for manufacturing an adhesive structure, the method comprising:
[0502] discharging an adhesive portion forming ink for forming an adhesive portion to be bonded to a contact object from a nozzle to pattern the adhesive portion, and
[0503] A low elastic portion forming ink for forming a low elastic portion having an elastic modulus lower than that of the adhesive portion is discharged from a nozzle to pattern the low elastic portion.
[0504] <19>
[0505] according to <18> The method for manufacturing the adhesive structure further includes discharging the heat conduction portion forming ink for forming the heat conduction portion from a nozzle to form the heat conduction portion continuously in the thickness direction of the adhesive structure.
[0506] <20>
[0507] according to <19> The method for producing the adhesive structure, wherein:
[0508] The heat transfer portion forming ink contains metal nanoparticles, and
[0509] The method further includes sintering the metal nanoparticles after discharging the heat conduction portion forming ink.
[0510] <21>
[0511] A method for manufacturing an electronic component, the method comprising: <1> ~ <9> The adhesive structure fixing element described in any one of the above.
[0512] <22>
[0513] according to <21> The method for manufacturing an electronic component, wherein:
[0514] The adhesive structure is a resist; and
[0515] The method further comprises:
[0516] On the substrate at a position corresponding to the first region as the edge portion of the obtained resist pattern, an adhesive portion forming ink for forming an adhesive portion to be bonded to a contact object is discharged from a nozzle, the adhesive portion is provided, and a first resist layer is formed;
[0517] On the substrate at a position corresponding to a second region different from the first region, a low elastic portion forming ink for forming a low elastic portion having a smaller elastic modulus than the adhesive portion is discharged from a nozzle, the low elastic portion is patterned and disposed, and a second resist layer is formed; and
[0518] curing the first resist layer and the second resist layer to form a resist pattern,
[0519] The discharge of the adhesive portion forming ink and the discharge of the low elastic portion forming ink include:
[0520] The adhesive portion forming ink and the low elastic portion forming ink are simultaneously provided on the substrate, and
[0521] A resist pattern is formed in which a portion corresponding to a first region of the resist pattern formed by the adhesive portion forming ink and a portion corresponding to a second region of the resist pattern formed by the low elastic portion forming ink are connected.
[0522] according to <1> ~ <9> Any one of the adhesive structures according to <10> The transfer adhesive layer, according to <11> ~ <17> Any one of the electronic components according to <18> ~ <20> The method for producing an adhesive structure according to any one of the above <21> ~ <22> The method for manufacturing an electronic component described in any one of the above can solve various conventional problems and achieve the purpose of the present invention.
[0523] The above embodiments are illustrative and do not limit the present invention. Therefore, many additional modifications and variations are possible based on the above teachings. For example, within the scope of the present invention, the elements and / or features of different illustrative embodiments can be combined and / or replaced with each other. Any of the above operations can be performed in various other ways, such as in an order different from the above order.
[0524] This application is based on and claims the benefit of priority of Japanese Patent Applications No. 2022-044905 and No. 2022-190614 filed with the Japan Patent Office on March 22, 2022 and November 29, 2022, respectively, the entire contents of which are incorporated herein by reference.
[0525] Reference numerals list
[0526] 1. Adhesion
[0527] 2 Low elasticity part
[0528] 3. Heat transfer part
[0529] 4 Wire bonding contacts
[0530] 10 Adhesive layer
[0531] 20 substrate
[0532] 30 Heating element
[0533] 30-1 Heating element
[0534] 30-2 Heating element
[0535] 40 Cooling element
[0536] 50 Middle Layer
[0537] 60 Wiring
[0538] 100 Conventional adhesive layer
[0539] 101 Conventional bonding
[0540] 102 Conventional low elasticity
[0541] 200 Silicon substrate
[0542] 300 Printed Wiring Board (PWB) Substrate
[0543] 501 Electrode
[0544] 502 Electrode
Claims
1. An adhesive structure comprising: Adhesion portion that adheres to a contact object; as well as a low elastic portion having an elastic modulus lower than that of the adhesive portion, Here, at least one of the adhesive portion and the low elastic portion has a pattern shape.
2. The adhesive structure according to claim 1, wherein The adhesive structure is a layered adhesive structure.
3. The adhesive structure according to claim 1 or 2, wherein: The shape and size of a portion of the adhesive portion and a portion of the low-elastic portion exposed on one surface are different from the shape and size of another portion of the adhesive portion and another portion of the low-elastic portion exposed on the other surface.
4. The adhesive structure according to any one of claims 1 to 3, wherein At least one of the adhesive portion and the low-elastic portion has a size of 10 μm or more in the planar direction of the adhesive structure.
5. The adhesive structure according to any one of claims 1 to 4, wherein The volume ratio of the low elastic part to the adhesive structure is 5% to 90%.
6. The adhesive structure according to any one of claims 1 to 5, wherein The elastic modulus of the low elastic portion is 70% or less of the elastic modulus of the bonding portion.
7. The adhesive structure according to any one of claims 1 to 6, wherein The elastic modulus of the low elastic portion is 3000 MPa or less. 8 . The adhesive structure according to claim 1 , further comprising a heat conductive portion continuous in the thickness direction.
9. The adhesive structure according to any one of claims 1 to 8, wherein At least one of the adhesive portion and the low elastic portion contains a photocurable resin.
10. An adhesive layer for transfer, comprising: Temporary support; as well as The adhesive structure according to any one of claims 1 to 9, which is a layered adhesive structure on the temporary support.
11. An electronic component comprising the adhesive structure according to any one of claims 1 to 9.
12. The electronic component according to claim 11, further comprising: first element; as well as A second element is fixed to the first element by the adhesive structure.
13. The electronic component according to claim 12, wherein: A difference in linear thermal expansion coefficient between the first element and the second element is 0 ppm / K to 20 ppm / K.
14. The electronic component according to claim 12 or 13, wherein: The first element is a heating element or a cooling element, and the second element is a substrate.
15. The electronic component according to any one of claims 12 to 14, wherein: The first element is a semiconductor.
16. A method for producing an adhesive structure, the method comprising: discharging an adhesive portion forming ink for forming an adhesive portion to be bonded to a contact object from a nozzle to pattern the adhesive portion, and A low elastic portion forming ink for forming a low elastic portion having an elastic modulus lower than that of the adhesive portion is discharged from a nozzle to pattern the low elastic portion. 17 . The method for manufacturing an adhesive structure according to claim 16 , further comprising discharging the heat conduction portion forming ink for forming the heat conduction portion from a nozzle to form the heat conduction portion continuously in a thickness direction of the adhesive structure.
18. The method for producing an adhesive structure according to claim 17, wherein: The heat transfer portion forming ink contains metal nanoparticles, and The method further includes sintering the metal nanoparticles after discharging the heat conduction portion forming ink.
19. A method of manufacturing an electronic component, the method comprising fixing the component by using the adhesive structure according to any one of claims 1 to 9.
20. The method for manufacturing an electronic component according to claim 19, wherein: The adhesive structure is a resist; as well as The method further comprises: On the substrate at a position corresponding to the first region as the edge portion of the obtained resist pattern, an adhesive portion forming ink for forming an adhesive portion to be bonded to a contact object is discharged from a nozzle, the adhesive portion is provided, and a first resist layer is formed; On the substrate at a position corresponding to a second region different from the first region, a low elastic portion forming ink for forming a low elastic portion having a smaller elastic modulus than the adhesive portion is discharged from a nozzle, the low elastic portion is patterned and disposed, and a second resist layer is formed; and curing the first resist layer and the second resist layer to form a resist pattern, The discharge of the adhesive portion forming ink and the discharge of the low elastic portion forming ink include: The adhesive portion forming ink and the low elastic portion forming ink are simultaneously provided on the substrate, and A resist pattern is formed in which a portion corresponding to a first region of the resist pattern formed by the adhesive portion forming ink and a portion corresponding to a second region of the resist pattern formed by the low elastic portion forming ink are connected.