Elastin-like polypeptide adhesive patch as well as preparation method and application thereof

CN118924941APending Publication Date: 2024-11-12SHANGPU BOYUAN (BEIJING) BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975921.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

但由于现有的组织粘合剂还存在诸多缺点,例如粘合强度低 、弹性较差、生物相容性与可降解性较低等,使得新型组织粘合剂的研发变得十分迫切

Benefits of technology

(1)本发明以生物相容性的类弹性蛋白多肽为基础,通过化学改性赋予其光交联能力,同时添加丙烯酸,丙烯酸-N-羟基琥珀酰亚胺酯和光引发剂,进而光交联制备了一种类弹性蛋白多肽粘附贴片,其具有操作简便、粘附迅速、粘合力强、生物相容性和可降解性好、弹性优异等诸多优势。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118924941A_ABST
    Figure CN118924941A_ABST
Patent Text Reader

Abstract

The invention provides an elastin-like polypeptide adhesive patch as well as a preparation method and application thereof. The method comprises the following steps: (1) reacting elastin-like polypeptide with a modifier to obtain modified elastin-like polypeptide; and (2) dissolving the modified elastin-like polypeptide in water, adding acrylic acid, acrylic acid-N-succinimide ester and a photoinitiator, mixing, and carrying out a photo-crosslinking reaction to obtain the elastin-like polypeptide adhesion patch, the amino acid sequence of the elastin-like polypeptide is as shown in SEQ ID NO: 1. The method is simple in process, raw materials are easy to obtain, reaction conditions are mild, and the prepared elastin-like polypeptide adhesion patch has excellent adhesion performance, biocompatibility, degradability and elasticity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of biomedical materials, and in particular to an elastin-like polypeptide adhesive patch and a preparation method and application thereof. Background Art

[0002] At present, sutures and staples are mostly used clinically to achieve wound closure or implant fixation. These traditional invasive treatment methods are not only complicated to operate and time-consuming, but may also cause secondary damage to fragile tissues, causing greater pain to patients. If the wound is not properly treated, there will be consequences such as wound infection and cracking, and obvious scars will be left after surgery. The concept of modern medicine is to minimize the patient's pain, let the patient recover as soon as possible, and while restoring the function to the greatest extent, it is hoped that the appearance can also be perfectly restored. Therefore, clinical needs continue to promote the rapid development of tissue adhesion materials, and their application as skin, blood vessels, organs and hemostatic adhesion materials in medicine is becoming more and more extensive. Tissue adhesives, as a new type of adhesive material, have broad application potential in clinical practice. In terms of chemical composition, the adhesives currently used in clinical practice are divided into three categories: cyanoacrylate adhesives, gelatin-resorcinol-formaldehyde adhesives, and fibrin adhesives. However, due to the many disadvantages of existing tissue adhesives, such as low bonding strength, poor elasticity, low biocompatibility and low degradability, the research and development of new tissue adhesives has become very urgent. Summary of the invention

[0003] The present invention aims to solve one of the technical problems in the prior art at least to a certain extent. To this end, one object of the present invention is to provide an elastin-like polypeptide adhesive patch and a preparation method and application thereof.

[0004] In a first aspect of the present invention, the present invention provides a method for preparing an elastin-like polypeptide adhesive patch. According to an embodiment of the present invention, the method comprises: (1) reacting the elastin-like polypeptide with a modifier to obtain a modified elastin-like polypeptide; (2) dissolving the modified elastin-like polypeptide in water, adding acrylic acid, acrylic acid-N-succinimidyl ester and a photoinitiator, and mixing them to perform a photocrosslinking reaction to obtain an elastin-like polypeptide adhesive patch; The amino acid sequence of the elastin-like polypeptide is shown in SEQ ID NO:1.

[0005] According to the method for preparing an elastin-like polypeptide adhesive patch according to the above embodiment of the present invention, the elastin-like polypeptide is reacted with a modifier, and the elastin-like polypeptide is given photocrosslinking ability through chemical modification. The modified elastin-like polypeptide is then dissolved in water, and acrylic acid, acrylic acid-N-succinimide ester and a photoinitiator are added and mixed to perform a photocrosslinking reaction. Under the action of the photoinitiator, the modified elastin-like polypeptide, acrylic acid, and acrylic acid-N-succinimide ester are crosslinked to form an interpenetrating network structure. The elastin-like polypeptide has good elasticity and biocompatibility, and polyacrylic acid has good biocompatibility and stability, and its surface contains a large number of carboxyl groups, which can be quickly and strongly adhered to the tissue surface through hydrogen bonds. The modified elastin-like polypeptide and acrylic acid crosslinking combine to give the adhesive patch a fast and strong adhesion ability as well as good mechanical properties, biocompatibility and elasticity.

[0006] In addition, the elastin-like polypeptide adhesive patch according to the above embodiment of the present invention also has the following technical features: In some embodiments of the present invention, in step (1), the molar ratio of the elastin-like polypeptide to the modifier is 1:(0.2-50).

[0007] In some embodiments of the present invention, the modifier includes at least one of methacrylic acid-N-hydroxysuccinic acid imide ester and methacrylic anhydride.

[0008] In some embodiments of the present invention, in step (1), the reaction temperature is 2-20° C. and the reaction time is 2-48 h.

[0009] In some embodiments of the present invention, step (1) further comprises: dialyzing the elastin-like polypeptide after reacting it with the modifier.

[0010] In some embodiments of the present invention, in step (2), the molar ratio of the modified elastin-like polypeptide, the acrylic acid, the acrylic acid-N-succinimidyl ester and the photoinitiator is 1: (0.01-50): (0.01-10): (0.01-1).

[0011] In some embodiments of the present invention, in step (2), the mixing temperature is 4°C to 40°C.

[0012] In some embodiments of the present invention, the wavelength used in the photo-crosslinking reaction is 365nm~405nm.

[0013] In some embodiments of the present invention, the photo-crosslinking reaction time is 1 min to 30 min.

[0014] In some embodiments of the present invention, the photoinitiator includes at least one of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone, phenyl (2,4,6-trimethylbenzoyl) phosphate lithium salt and α-ketoglutaric acid.

[0015] In a second aspect of the present invention, the present invention provides an elastin-like polypeptide adhesive patch. According to an embodiment of the present invention, the elastin-like polypeptide adhesive patch is obtained by the above method.

[0016] In a third aspect of the present invention, the present invention proposes the use of the above-mentioned elastin-like polypeptide adhesive patch in the field of biomaterial engineering, biomedical engineering, medicine, and environment.

[0017] The present invention has at least the following technical effects: (1) The present invention is based on a biocompatible elastin-like polypeptide, which is endowed with photocrosslinking ability through chemical modification, and acrylic acid, acrylic acid-N-hydroxysuccinimide ester and a photoinitiator are added to prepare an elastin-like polypeptide adhesive patch through photocrosslinking. The elastin-like polypeptide adhesive patch has many advantages such as simple operation, rapid adhesion, strong adhesion, good biocompatibility and degradability, and excellent elasticity.

[0018] (2) From the perspective of material source, elastin-like polypeptide is an important extracellular matrix protein. Its main function is to give the tissue or organ in which it is located elasticity and reversible deformation ability. It has good elasticity and biocompatibility, and its application in tissue engineering has great potential. Polyacrylic acid has good biocompatibility and stability, and its surface contains a large number of carboxyl groups, which can quickly and strongly adhere to the tissue surface through hydrogen bonds. The combination of elastin-like polypeptide and polyacrylic acid forms an interpenetrating network structure, which gives the adhesive patch fast and strong adhesion ability as well as good mechanical properties and biocompatibility.

[0019] (3) From the perspective of preparation process and presentation form, the adhesive patch prepared by the present invention has a simple process and low production cost. Compared with traditional adhesive gels, the patch form of the present application greatly reduces the technical difficulty and inconvenience caused by the storage, use and in-situ adhesion of adhesive gels. It has opened up a new way to solve the defects of traditional sutures, staples and surgical adhesives, and has great potential in many medical fields such as wound sealing, tissue repair and sutureless wound closure. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 is the hydrogen spectrum of the modified elastin-like polypeptide of Example 1 of the present invention; Figure 2 This is a physical picture of the elastin-like polypeptide adhesive patch of Example 1 of the present invention; Figure 3 This is a graph showing the elasticity test results of the elastin-like polypeptide adhesive patch of Example 1 of the present invention; Figure 4 This is a graph showing the adhesion performance test results of the elastin-like polypeptide adhesive patch of Example 1 of the present invention; Figure 5 This is a microscopic photograph of fibroblasts cultured on the elastin-like polypeptide adhesive patch of Example 1 of the present invention; Figure 6 This is a diagram showing the cell compatibility test results of the elastin-like polypeptide adhesive patch of Example 1 of the present invention. DETAILED DESCRIPTION

[0022] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0023] In a first aspect of the present invention, the present invention provides a method for preparing an elastin-like polypeptide adhesive patch. According to an embodiment of the present invention, the method comprises: S100: Reacting elastin-like peptides with modifiers

[0024] In this step, the elastin polypeptide is dissolved in water, and then a modifier is added to react, thereby giving the elastin-like polypeptide photo-crosslinking ability through chemical modification. It should be noted that the amount of water added is not particularly limited, and it is only necessary to dissolve the elastin-like polypeptide.

[0025] According to an embodiment of the present invention, the modifier includes at least one of methacrylic acid-N-hydroxysuccinic acid imide ester and methacrylic anhydride. The inventors found that the above modifier can achieve smooth modification of elastin-like polypeptides to obtain modified elastin polypeptides.

[0026] According to an embodiment of the present invention, the molar ratio of the elastin-like polypeptide to the modifier is 1:(0.2-50). For example, the molar ratio of the elastin-like polypeptide to the modifier is 1:0.2, 1:1, 1:2, 1:5, 1:10, 1:15, 1:20, 1:30, 1:40, 1:40, etc., or any range between the above two data. The inventors have found that the molar ratio of the elastin-like polypeptide to the modifier is controlled within the above range, which can better achieve the modification of the elastin-like polypeptide and improve the yield of the modified elastin-like polypeptide.

[0027] According to an embodiment of the present invention, the reaction temperature is 2-20°C, and the reaction time is 2-48h. For example, the reaction temperature is 2°C, 5°C, 7°C, 10°C, 12°C, 15°C, 18°C, 20°C, etc., and the reaction time is 2h, 5h, 10h, 15h, 20h, 30h, 40h, 48h, etc. The inventors have found that controlling the reaction temperature and time within the above range can make the elastin-like polypeptide easier to modify, improve the modification efficiency of the elastin-like polypeptide, and improve the yield of the modified elastin-like polypeptide.

[0028] According to an embodiment of the present invention, S100 further includes: dialyzing the elastin-like polypeptide after reacting with the modifier. After the elastin-like polypeptide reacts with the modifier, unreacted raw materials or other impurities may exist. After the reaction, a modified elastin-like polypeptide with higher purity may be obtained by dialysis. It should be noted that dialysis is a conventional operation in the art, and those skilled in the art may select specific dialysis conditions according to actual conditions. Furthermore, after dialysis, freeze-drying may be performed to obtain a pure modified elastin-like polypeptide.

[0029] S200: Preparation of elastin-like polypeptide adhesive patches

[0030] In this step, after the modified elastin polypeptide is dissolved in water, acrylic acid, acrylic acid-N-succinimide ester and photoinitiator are added and mixed to perform a photocrosslinking reaction. Under the action of the photoinitiator, the modified elastin polypeptide, acrylic acid, and acrylic acid-N-succinimide ester are cross-linked to form an interpenetrating network structure. The elastin polypeptide has good elasticity and biocompatibility, and polyacrylic acid has good biocompatibility and stability. Its surface contains a large number of carboxyl groups, which can adhere quickly and strongly to the tissue surface through hydrogen bonds. The modified elastin polypeptide and acrylic acid cross-linking combine to give the adhesive patch fast and strong adhesion as well as good mechanical properties, biocompatibility and elasticity. It should be noted that the amount of water used is not particularly limited, and the modified elastin polypeptide only needs to be dissolved.

[0031] The amino acid sequence of the elastin-like polypeptide is [(VPGVG)2VPGKG(VPGVG)2] 25(SEQ ID NO: 1).

[0032] (SEQ ID NO: 1).

[0033] According to an embodiment of the present invention, the modified elastin-like polypeptide is dissolved in water, acrylic acid, acrylic acid-N-succinimidyl ester and a photoinitiator are added, mixed and poured into a mold, and then subjected to a photocrosslinking reaction to obtain an elastin-like polypeptide adhesive patch of a specific shape. The mold can be selected according to actual needs, for example, the mold includes a rectangular, square, circular, etc.

[0034] According to an embodiment of the present invention, the molar ratio of the modified elastin-like polypeptide, acrylic acid, acrylic acid-N-succinimidyl ester and the photoinitiator is 1: (0.01-50): (0.01-10): (0.01-1). The inventors have found that by controlling the molar ratio of the modified elastin-like polypeptide, acrylic acid, acrylic acid-N-succinimidyl ester and the photoinitiator within the above range, a better cross-linking effect can be achieved and a higher mechanical strength can be achieved.

[0035] According to an embodiment of the present invention, the mixing temperature is 4°C to 40°C. For example, the mixing temperature is 4°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, etc., or a range between any two of the above data. By controlling the mixing temperature within the above range, more sufficient mixing can be achieved to achieve a more uniform cross-linking effect.

[0036] According to an embodiment of the present invention, the wavelength used for the photocrosslinking reaction is 365nm~405nm. For example, the wavelength of the crosslinking is 365nm, 370nm, 375nm, 380nm, 385nm, 395nm, 405nm, etc., or a range between any two of the above data points. By controlling the wavelength within the above range, the components can be fully crosslinked to obtain an elastin-like polypeptide adhesive patch with excellent performance. Furthermore, the time of the photocrosslinking reaction is 1min~30min.

[0037] According to an embodiment of the present invention, the photoinitiator includes at least one of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator 2959), phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (photoinitiator LAP) and α-ketoglutaric acid.

[0038] In a second aspect of the present invention, the present invention provides an elastin polypeptide-like adhesive patch. According to an embodiment of the present invention, the elastin polypeptide-like adhesive patch is obtained by the above method. Thus, the elastin polypeptide-like adhesive patch has excellent adhesion performance, biocompatibility, degradability and elasticity.

[0039] In a third aspect of the present invention, the present invention proposes the use of the above-mentioned elastin-like polypeptide adhesive patch in the field of biomaterial engineering, biomedical engineering, medicine, and environment.

[0040] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0041] Example 1

[0042] (1) Using elastin-like polypeptide (SEQ ID NO: 1) as raw material, 0.1 mol of elastin-like polypeptide was fully dissolved in 50 mL of deionized water, and then 0.5 mol of methacrylic acid-N-hydroxysuccinic acid imide was added, and the mixture was stirred at 15°C for 12 h. After the reaction, the mixture was dialyzed in deionized water for 3 days and freeze-dried to obtain a white flocculent methacrylic acid-modified elastin-like polypeptide. The H NMR spectrum results of the prepared methacrylic acid-modified elastin-like polypeptide are shown in Figure 1 .from Figure 1Yes, the elastin-like polypeptide was modified successfully.

[0043] (2) Dissolve 1 mol of methacrylic acid-modified elastin-like polypeptide in 10 mL of deionized water and stir thoroughly until completely dissolved. Then add 0.3 mol of acrylic acid, 0.1 mol of acrylic acid-N-succinimidyl ester, and 0.05 mol of photoinitiator 2959 and stir vigorously at 25°C until completely dissolved. The mixed system is the pre-crosslinking solution.

[0044] (3) Take 2 mL of the pre-crosslinking solution and pour it into a rectangular molding mold, then irradiate with 365 nm ultraviolet light for 20 min, take out the crosslinked adhesive patch, and you can get an elastin-like polypeptide adhesive patch with rapid adhesion, high adhesion strength and good biocompatibility. Figure 2 shown.

[0045] The adhesion performance, elasticity and biocompatibility of the elastin-like polypeptide adhesive patch prepared in Example 1 were tested as follows: (1) Take a piece of elastin polypeptide adhesive patch (area 1cm×5cm) and place it on the surface of two fingers. It can instantly exert adhesion and then stretch to both sides. Its stretched length can reach 8 times its original length. Figure 3 As shown, it is shown that the elastin-like polypeptide adhesive patch of the present application has excellent mechanical properties and good elasticity.

[0046] (2) Take a piece of elastin peptide adhesive patch (area 1cm×1cm) and stick it on the surface of pig skin, then press a weight on the other side of the adhesive patch for 2 seconds. The adhesive force generated by this can lift a weight of at least 200g. Figure 4 As shown, it is shown that the elastin-like polypeptide adhesive patch of the present application has rapid adhesion and excellent adhesion strength.

[0047] (3) Before planting fibroblasts, soak the adhesive patch in 75% ethanol overnight for disinfection, then wash the ethanol with PBS and soak it in RPMI 1640 medium for 2 hours. Then, mouse fibroblasts L929 were planted on the surface of the patch at a density of 1×106 cells / mL, and then cultured in an incubator at 37°C and 5% CO2. After 3 days, the cells were stained with the Calcein-AM live cell detection kit (Beyotime Biotechnology / Biyuntian Biotechnology Co., Ltd.) to observe cell morphology and take pictures. The results are shown in Figure 5 ,from Figure 5 It can be seen that the fibroblasts have grown into a distinct spindle-shaped state, demonstrating the good cell compatibility of the adhesion patch.

[0048] (4) The standard Calcein-AM live-dead cell detection kit (Beyotime Biotechnology / Biyuntian Biotechnology Co., Ltd.) was used to detect and calculate the cell survival rate. The results are shown in Figure 6 ,from Figure 6 It can be seen that the survival rate of cells is above 90%, indicating that the elastin-like polypeptide adhesive patch of the present application has excellent biocompatibility.

[0049] Example 2

[0050] (1) Using elastin-like polypeptide (SEQ ID NO: 1) as raw material, 1 mol of elastin-like polypeptide was fully dissolved in 100 mL of deionized water, and then 1 mol of methacrylic acid-N-hydroxysuccinic acid imide was added, and stirred at 8°C for 24 hours. After the reaction, the mixture was dialyzed in deionized water for 3 days and freeze-dried to obtain a white flocculent methacrylic acid-modified elastin-like polypeptide.

[0051] (2) Dissolve 1 mol of methacrylic acid-modified elastin-like polypeptide in 20 mL of deionized water and stir thoroughly until completely dissolved. Then add 1.5 mol of acrylic acid, 0.2 mol of acrylic acid-N-succinimidyl ester, and 0.1 mol of photoinitiator (α-ketoglutaric acid) and stir vigorously at 25 °C until completely dissolved. The mixed system is the pre-crosslinking solution.

[0052] (3) Take 1 mL of the above pre-crosslinking solution and pour it into a rectangular molding mold, then irradiate it with 365 nm ultraviolet light for 3 minutes, and take out the cross-linked adhesive patch to obtain an elastin-like polypeptide adhesive patch with rapid adhesion, high adhesion strength and good biocompatibility.

[0053] The performance test method of the elastin-like polypeptide adhesive patch obtained in Example 2 is the same as that in Example 1. The elastic performance test results show that the stretching length of the elastin-like polypeptide adhesive patch can reach 8 times the original length, the adhesive force can lift a weight of at least 210g, and the cell survival rate is above 90%. The performance of the elastin-like polypeptide adhesive patch obtained in Example 2 is close to that of Example 1.

[0054] Example 3

[0055] (1) Using elastin-like polypeptide (SEQ ID NO: 1) as raw material, 1 mol of elastin-like polypeptide was fully dissolved in 100 mL of deionized water, and then 10 mol of methacrylic acid-N-hydroxysuccinic acid imide was added, and stirred at 16°C for 40 hours. After the reaction, the mixture was dialyzed in deionized water for 3 days and freeze-dried to obtain a white flocculent methacrylic acid-modified elastin-like polypeptide.

[0056] (2) Dissolve 1 mol of methacrylic acid-modified elastin-like polypeptide in 20 mL of deionized water and stir thoroughly until completely dissolved. Then add 10 mol of acrylic acid, 5 mol of acrylic acid-N-succinimidyl ester, and 0.5 mol of photoinitiator (α-ketoglutaric acid) and stir vigorously at 25 °C until completely dissolved. The mixed system is the pre-crosslinking solution.

[0057] (3) Take 1 mL of the above pre-crosslinking solution and pour it into a rectangular molding mold, then irradiate it with 365 nm ultraviolet light for 15 min, and take out the cross-linked adhesive patch to obtain an elastin-like polypeptide adhesive patch with rapid adhesion, high adhesion strength and good biocompatibility.

[0058] The performance test method of the elastin-like polypeptide adhesive patch obtained in Example 3 is the same as that in Example 1. The elastic performance test results show that the stretching length of the elastin-like polypeptide adhesive patch can reach 9 times the original length, the adhesive force can lift a weight of at least 230g, and the cell survival rate is above 90%.

[0059] Example 4

[0060] (1) Using elastin-like polypeptide (SEQ ID NO: 1) as raw material, 1 mol of elastin-like polypeptide was fully dissolved in 100 mL of deionized water, and then 20 mol of methacrylic acid-N-hydroxysuccinic acid imide was added, and stirred at 5°C for 45 hours. After the reaction, the mixture was dialyzed in deionized water for 3 days and freeze-dried to obtain a white flocculent methacrylic acid-modified elastin-like polypeptide.

[0061] (2) Dissolve 1 mol of methacrylic acid-modified elastin-like polypeptide in 20 mL of deionized water and stir thoroughly until completely dissolved. Then add 20 mol of acrylic acid, 8 mol of acrylic acid-N-succinimidyl ester, and 0.8 mol of photoinitiator (α-ketoglutaric acid) and stir vigorously at 25 °C until completely dissolved. The mixed system is the pre-crosslinking solution.

[0062] (3) Take 1 mL of the above pre-crosslinking solution and pour it into a rectangular molding mold, then irradiate it with 365 nm ultraviolet light for 30 min, and take out the cross-linked adhesive patch to obtain an elastin-like polypeptide adhesive patch with rapid adhesion, high adhesion strength and good biocompatibility.

[0063] The performance test method of the elastin-like polypeptide adhesive patch obtained in Example 4 is the same as that in Example 1. The elastic performance test results show that the stretching length of the elastin-like polypeptide adhesive patch can reach 8 times the original length, the adhesive force can lift a weight of at least 200g, and the cell survival rate is above 90%.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an elastin-like polypeptide adhesive patch, It is characterized in that include: (1) reacting the elastin-like polypeptide with a modifier to obtain a modified elastin-like polypeptide; (2) dissolving the modified elastin-like polypeptide in water, adding acrylic acid, acrylic acid-N-succinimidyl ester and a photoinitiator, and mixing them to perform a photocrosslinking reaction to obtain an elastin-like polypeptide adhesive patch; The amino acid sequence of the elastin-like polypeptide is shown in SEQ ID NO:

1.

2. The method according to claim 1, It is characterized in that In step (1), the molar ratio of the elastin-like polypeptide to the modifier is 1:(0.2-50).

3. The method according to claim 1 or 2, It is characterized in that The modifier includes at least one of methacrylic acid-N-hydroxysuccinic acid imide ester and methacrylic anhydride.

4. The method according to claim 1 or 2, It is characterized in that In step (1), the reaction temperature is 2-20°C and the reaction time is 2-48h.

5. The method according to claim 1 or 2, It is characterized in that Step (1) further comprises: dialyzing the elastin-like polypeptide after reacting with the modifier.

6. The method according to claim 1, It is characterized in that In step (2), the molar ratio of the modified elastin-like polypeptide, the acrylic acid, the acrylic acid-N-succinimidyl ester and the photoinitiator is 1: (0.01-50): (0.01-10): (0.01-1).

7. The method according to claim 1 or 6, It is characterized in that In step (2), the mixing temperature is 4°C to 40°C; And / or, the wavelength adopted by the photo-crosslinking reaction is 365nm~405nm; And / or, the photo-crosslinking reaction time is 1 min to 30 min.

8. The method according to claim 1 or 6, It is characterized in that The photoinitiator includes at least one of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone, phenyl (2,4,6-trimethylbenzoyl) phosphate lithium salt and α-ketoglutaric acid.

9. An elastin-like polypeptide adhesive patch, It is characterized in that The method is obtained by any one of claims 1 to 8.

10. Use of the elastin-like polypeptide adhesive patch according to claim 9 in the fields of biomaterial engineering, biomedical engineering, medicine, and environment.