Mixed matrix membrane for selective ion separation and application thereof

By adding PCC-67 nanoparticles to the poly(biphenylpiperidine) matrix membrane to construct a hybrid matrix membrane, the problem of difficult to take into account in the prior art is solved, and efficient selection of monopolyvalent cations is achieved It is suitable for industrial waste liquid recycling and seawater resource utilization.

CN118925516AActive Publication Date: 2024-11-12ANHUI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411180100.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

While increasing the ion flux, existing mixed matrix membranes are difficult to maintain high monopolyvalent ion selectivity, resulting in low ion recovery efficiency and poor selective separation effect in applications.

Method used

PCC-67 nanoparticles were added to the quaternized poly(biphenylpiperidine) matrix membrane as filler, and the mixed matrix membrane was constructed by blending method, and the ion selectivity was improved using the metal organic coordination cage structure.

Benefits of technology

It realizes high selective separation under low fillers, significantly improves the recovery efficiency of single multivalent cations, and is suitable for industrial waste liquid recycling and comprehensive utilization of seawater resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011860800000051
    Figure BDA0005011860800000051
  • Figure BDA0005011860800000061
    Figure BDA0005011860800000061
  • Figure HDA0005011860810000011
    Figure HDA0005011860810000011
Patent Text Reader

Abstract

The invention discloses a mixed matrix membrane for selective ion separation and application of the mixed matrix membrane. The mixed matrix membrane is prepared by adding PCC-67 nanoparticles into a quaternized poly (biphenyl piperidine) matrix membrane as a filler. The mixed matrix membrane is constructed through a blending method, the process is simple, the repeatability is high, the obtained membrane has high monovalent and multivalent ion selectivity, high-selectivity separation of monovalent and multivalent cations can be achieved under the condition of low filler, the ion recovery efficiency is greatly improved, the application prospect is wide, and the method is suitable for industrial production. The method can be used for salt lake lithium extraction, seawater resource comprehensive utilization and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mixed matrix separation membranes, and in particular to a mixed matrix membrane for ion selective separation and application thereof. Background Art

[0002] With the continuous development of industry, the separation of cations of different valence states is very important in many special separation fields, such as the recovery of acid from industrial waste acid, the removal of heavy metal ions in wastewater, the extraction of lithium from salt lakes, and the comprehensive utilization of seawater resources. In recent years, the research on the preparation and performance of monovalent and polyvalent cation separation membranes has gradually increased, and more simple and efficient preparation methods have emerged, which have achieved certain results in their performance (mainly including flux and selectivity) and durability. However, most studies focus on improving selectivity, usually at the expense of monovalent permeability. Mixed matrix membranes (MMMs) are considered to be one of the most promising solutions to this contradiction due to their advantages of organic-inorganic component characteristics and adjustable physicochemical properties.

[0003] The article "Hybrid Cation exchange membranes with lithium ion-sieves for highly enhanced Li + A sulfonated polyetheretherketone (SPEEK)-based mixed matrix membrane with particulate lithium ion sieves HMO and HMO-S was fabricated in the paper. + The construction of selective transfer channels enables Li + The permeability of Li + / Mg 2+ , Li + / K + The permeation selectivity increased by about 5 times [1] The article “Highly efficient Li + / Mg 2+ In the paper "separation of monovalent cation permselective membrane enhanced by 2D metal organic framework nanosheets", Zn-TCPP was introduced into surface cross-linked sulfonated polyethersulfone (SPES) to prepare mixed matrix membranes. The obtained mixed matrix membranes were effective for Li + / Mg 2+ The selectivity is 8.99, Li + The permeation flux is 9.12×10 -9 mol cm -2 s-1[2] Although the above-mentioned mixed matrix membrane has improved ion flux due to the addition of nanoparticles, it has not achieved good results in selective separation of ions.

[0004] Metal-organic coordination cages, also known as metal coordination cage compounds, are materials that connect metal ions and organic ligands through coordination chemical bonds to form a three-dimensional cage structure. Using different ligands and different metal ions can produce many different structures. It has been proven that metal cage compounds have a wide range of applications in the field of supramolecular materials such as molecular recognition, gas adsorption, ion channel energy conversion, and catalytic reactions. However, research in the field of ion selective separation is still lacking.

[0005] References:

[0006] 1.J.Zhang,X.Cui,F.Yang,L.et al.Hybrid Cation exchange membranes with lithium ion-sieves for highly enhanced Li + permeation and permselectivity,Macromol.Mater.Eng.304(2019)1800567.

[0007] 2.Tao,Lu.Wang,X.Wu,F.et al.Highly efficient Li + / Mg 2+ separation of monovalent cation permselective membrane enhanced by 2D metal organicframework nanosheets.Separation and Purification Technology.296(2022):121309. Summary of the invention

[0008] On the basis of the above-mentioned prior art, the present invention provides a method for preparing a mixed matrix membrane for ion selective separation and its application, aiming to make it have high selectivity for monovalent and polyvalent ions while having high flux.

[0009] In order to achieve the above object, the present invention adopts the following technical solution:

[0010] The invention provides a mixed matrix membrane for ion selective separation. The mixed matrix membrane is prepared by adding PCC-67 nanoparticles (having a metal organic coordination cage structure) as fillers into a quaternized poly (biphenyl piperidine) matrix membrane.

[0011] The method for preparing the mixed matrix membrane of the present invention comprises the following steps:

[0012] 1) dissolving H3L in a mixture of DMF, ethanol and water to form solution A; dissolving holmium chloride hexahydrate in a mixture of DMF, ethanol and water to form solution B; mixing solution A and solution B, reacting, washing and drying the obtained product to obtain PCC-67 nanoparticles;

[0013] 2) mixing methyl iodide as a quaternizing agent with poly(biphenyl piperidine) in dimethyl sulfoxide, and performing a room temperature quaternization reaction in the dark to obtain a quaternized poly(biphenyl piperidine);

[0014] 3) adding PCC-67 nanoparticles and quaternized poly(biphenylpiperidine) into dimethyl sulfoxide and uniformly mixing them by ultrasonication to obtain a membrane solution, and then coating the membrane solution onto a glass plate and drying it to obtain a mixed matrix membrane.

[0015] As a further preferred embodiment of the present invention, in step 1), H3L is used as the organic ligand, hexahydrate and holmium chloride are used as the metal sources, and the molar ratio of H3L to holmium chloride hexahydrate is 1:3.

[0016] As a further preferred embodiment of the present invention, the specific process of step 1) is: adding H3L to a mixture of DMF, ethanol and water (the volume ratio of DMF, ethanol and water is 3:1:0.25), and ultrasonicating at room temperature for 5 to 15 minutes to form a solution A; adding holmium chloride hexahydrate to a mixture of DMF, ethanol and water (the volume ratio of DMF, ethanol and water is 3:1:0.25), and ultrasonicating at room temperature for 5 to 15 minutes to form a solution B; mixing solution A with solution B, ultrasonicating for 5 to 15 minutes to fully mix them, reacting at 70-80°C for 48-72 hours, and washing the obtained product with DMF and ethanol in turn, and then drying at 55-65°C to obtain PCC-67 nanoparticles.

[0017] As a further preferred embodiment of the present invention, in step 2), the usage ratio of poly(biphenylpiperidine) to methyl iodide is 1 g:320 μL, and the quaternization reaction time is 10-14 h.

[0018] As a further preferred technical solution of the present invention, in step 3), the mass ratio of PCC-67 nanoparticles to quaternized poly(biphenylpiperidine) is 5-10%:95-90%.

[0019] As a further preferred technical solution of the present invention, in step 3), the drying temperature is 60-80°C.

[0020] The mixed matrix membrane provided by the present invention can be used as a monovalent cation selective ion separation membrane, such as for recovering ions in industrial waste liquid.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0022] The present invention constructs a mixed matrix membrane through a blending method, and the process is simple and highly repeatable. The obtained membrane has high selectivity for monovalent and polyvalent ions, and can achieve highly selective separation of monovalent and polyvalent cations under low filler conditions, greatly improving the ion recovery efficiency. It has broad application prospects, such as lithium extraction from salt lakes and comprehensive utilization of seawater resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the structure of PCC-67 nanoparticles prepared in Example 1 of the present invention.

[0024] Figure 2 SEM images of the PCC-67 / QPBPIP mixed matrix membranes prepared in Examples 1 and 2 and the QPBPIP membrane prepared in Comparative Example 1, wherein (a) and (d) are the surface image and cross-sectional image of the pure QPBPIP membrane in Comparative Example 1 with a PCC-67 mass fraction of 0 wt%, respectively; (b) and (e) are the surface image and cross-sectional image of the mixed matrix membrane in Example 1 with a PCC-67 mass fraction of 5 wt%, respectively; (c) and (f) are the surface image and cross-sectional image of the mixed matrix membrane in Example 2 with a PCC-67 mass fraction of 10 wt%, respectively.

[0025] Figure 3 Infrared images of H3L, PCC-67 nanoparticles, QPBPIP membrane and PCC-67 / QPBPIP mixed matrix membrane prepared in Examples 1 and 2 and Comparative Example 1.

[0026] Figure 4 The flux of different ions and the separation selectivity of each ion pair of the PCC-67 / QPBPIP mixed matrix membrane prepared in Examples 1 and 2 and the QPBPIP membrane prepared in Comparative Example 1, wherein (a) corresponds to the QPBPIP membrane with a PCC-67 mass fraction of 0 wt% in Comparative Example 1, (b) corresponds to the mixed matrix membrane with a PCC-67 mass fraction of 5 wt% in Example 1, and (c) corresponds to the mixed matrix membrane with a PCC-67 mass fraction of 10 wt% in Example 2. DETAILED DESCRIPTION

[0027] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0028] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0029] Example 1

[0030] In this example, a mixed matrix membrane for ion selective separation was prepared according to the following steps:

[0031] (1) Preparation of PCC-67 nanoparticles

[0032] Preparation of H3L: L-phenylalanine methyl ester hydrochloride (16.5mmol) was added to dichloromethane (200mL), cooled to 0°C, triethylamine (4.5mL) was added, and then a dichloromethane solution (15mL) containing 1,3,5-benzenetricarboxylic acid chloride (5.5mmol) was added dropwise, and stirred at room temperature for 18 hours. After the reaction was completed, the precipitate was removed by filtration, and the remaining solution was washed twice with HCl solution (10mM) and deionized water in turn. The organic phase was collected and dried over anhydrous MgSO4 to obtain L-Me3. A solution of L-Me3 (3.69mmol) in methanol (100mL) was cooled to 0°C, and an aqueous sodium hydroxide solution (30mL, 2M) was added. The mixture was returned to room temperature, stirred for 22 hours, diluted with water (100mL), and then an aqueous HCl solution (2M) was added to adjust the pH to less than 3. After standing for 4 hours, the white precipitate was collected by filtration and dried in vacuo to obtain H3L.

[0033] Weigh 45 mg of holmium chloride hexahydrate (0.12 mmol) and 42 mg of propiolic acid in a 20 mL glass bottle, add 3 mL of DMF, 1 mL of ethanol and 0.25 mL of deionized water, and ultrasonicate for 10 min at room temperature to form a precursor metal center ion solution; weigh 26 mg of H3L (0.04 mmol) in a 20 mL glass bottle, add 3 mL of DMF, 1 mL of ethanol and 0.25 mL of deionized water, and ultrasonicate for 10 min at room temperature to form a ligand solution. Mix the metal center ion solution and the ligand solution and ultrasonicate for 10 min. Divide the mixed solution into ten equal parts and put them into 10 mL glass bottles, and react in a 70° oven for 48 h. The obtained product is centrifuged and washed three times with DMF and ethanol at 7500 rpm to remove unreacted products, and the obtained PCC-67 crystals are dried at 60°C in a high temperature drying oven for 12 h to obtain solid powder PCC-67 nanoparticles.

[0034] (2) Preparation of quaternized poly(biphenylpiperidine)

[0035] First, 1.54 g (10 mmol) of biphenyl and 1.343 mL (12 mmol) of N-methyl-4-piperidone were dissolved in 8.8 mL of dichloromethane, and 740 μL (10 mmol) of trifluoroacetic acid and 8.8 mL (100 mmol) of trifluoromethanesulfonic acid were added dropwise in an ice bath, and stirred for 6 hours under an ice bath to obtain a viscous dark red solution after the reaction. The obtained product was slowly poured into a 1 M NaOH aqueous solution to obtain a white fibrous product, which was washed with deionized water until neutral and dried to obtain a poly (biphenyl piperidine) copolymer (PBPIP).

[0036] 1.0 g of PBPIP was dissolved in 20 mL of dimethyl sulfoxide, and 320 μL (1.3 eq.) of iodomethane solution was added. The mixture was reacted at room temperature for 12 h in the dark to obtain an orange-red solution, which was poured into ethyl acetate to precipitate to obtain a yellow fibrous solid. The solid was washed with deionized water, filtered, and dried in a vacuum drying oven at 60°C to obtain a quaternized poly(biphenylpiperidine) copolymer (QPBPIP).

[0037] (3) Preparation of mixed matrix membranes

[0038] Weigh 95 mg of the quaternized poly(biphenyl piperidine) and 1.5 mL of dimethyl sulfoxide and add 5 mg of PCC-67 nanoparticles, then add them to QPBPIP, and ultrasonicate until they are evenly dispersed to obtain a membrane solution. The membrane solution is coated on a glass plate, and then transferred to a heating table and dried at 70°C for 6 hours to obtain a mixed matrix membrane with a PCC-67 nanoparticle addition amount of 5 wt%, also known as PCC-67 / QPBPIP mixed matrix membrane (hereinafter referred to as membrane in the test).

[0039] Example 2

[0040] In this example, a mixed matrix membrane was prepared in the same manner as in Example 1, except that in step 3), the mass of the quaternized poly(biphenylpiperidine) was 90 mg, the mass of the PCC-67 nanoparticles was 10 mg, and a mixed matrix membrane with a PCC-67 nanoparticle addition amount of 10 wt % was obtained.

[0041] Comparative Example 1

[0042] In this example, a membrane was prepared in the same manner as in Example 1, except that in step 3), the mass of the quaternized poly(biphenylpiperidine) was 100 mg, the mass of the PCC-67 nanoparticles was 0 mg, and a pure QPBPIP membrane with 0 wt % PCC-67 nanoparticles was obtained.

[0043] Figure 1 The schematic diagram of the structure of PCC-67 nanoparticles prepared in Example 1 shows that PCC-67 is a multi-level pore structure assembled from double-walled octahedral cages. It has two different pore environments: the internal cavity (1.5 nm) of the coordination cage and the external cavity (2.4 nm) formed by its spatial stacking. The spatial stacking pattern of PCC-67 is relatively tight.

[0044] Figure 2 The SEM images of the PCC-67 / QPBPIP mixed matrix membranes prepared in Examples 1 and 2 and the QPBPIP membrane prepared in Comparative Example 1 show that the PCC-67 nanoparticles are evenly dispersed in the membranes, and the cross-sectional structure of the membranes is uniform and continuous without obvious membrane gaps.

[0045] Figure 3 The infrared images of H3L, PCC-67 nanoparticles, QPBPIP membrane and PCC-67 / QPBPIP mixed matrix membrane prepared in Examples 1 and 2 and Comparative Example 1. The ligand H3L has a wavelength of 3305 cm -1 The absorption peak of hydroxyl group appears around 2925cm -1 and 1728cm -1 The absorption vibration peaks of carboxyl groups appear at 3300 cm-1, and the peaks of PCC-67 at these three locations have different degrees of change. -1 The absorption peak of hydroxyl group at 2925cm -1 and 1728cm -1 The absorption vibration peak of the carboxyl group almost disappeared, indicating that the carboxyl group of the ligand H3L and the metal atom were successfully coordinated, and the remaining peaks of the ligand also had different degrees of shift, which was caused by the energy transfer during the coordination process. The same changes can be seen in the mixed matrix membrane.

[0046] The membranes obtained from the above-mentioned embodiments and comparative examples were subjected to the following ion separation performance tests:

[0047] The electrodialysis device consists of two polar chambers, a desalination chamber and a concentration chamber. 2 ) PCC-67 / QPBPIP mixed matrix membrane or pure QPBPIP membrane is placed in the center of the electrodialysis device to separate the concentration chamber from the desalination chamber, and an anion exchange membrane is used to separate the polar chamber from the desalination chamber and the polar chamber from the concentration chamber. The current density is 2 mA cm -2 , an electrodialysis test was performed for a specific duration (1 h).

[0048] Test K + / Mg 2+ 、Na + / Mg 2+ and Li+ / Mg 2+ The electrically driven cation permselective performance of the three separation systems. + / Mg 2+ Separation system, desalination chamber contains 100mL of 0.1mol L -1 KC1 and 0.1 mol L -1 MgCl2 solution, and the concentrating compartment contained 100 mL of deionized water. + / Mg 2+ Separation system, desalination chamber contains 100mL of 0.1mol L -1 NaCl and 0.1 mol L -1 MgCl2 solution, and the concentrating compartment contained 100 mL of deionized water. + / Mg 2+ Separation system, desalination chamber contains 100mL of 0.1mol L -1 LiC1 and 0.1 mol L -1 MgCl2 solution, while the concentrating compartment contained 100 mL of deionized water. In addition, 100 mL of 0.3 mol L -1 The Na2SO4 solution is supplied to the two electrode chambers. After 1 hour of electrodialysis test, samples are drawn from the concentration chamber to test the concentration of cations in the separation system. The concentration of cations is measured by an inductively coupled plasma emission spectrometer (ICP-AES).

[0049] The flux of cations passing through the membrane is calculated by the change in cation concentration in the concentration chamber before and after the test. The calculation formula is as follows:

[0050]

[0051] Among them, J N n+ is the flux of cations through the membrane (mol h -1 m -2 ), C0 and C t (mol L -1 ) are the initial concentration (t=0 h) and the cation concentration at the end of the electrodialysis test, V is the volume of the solution in the concentrating compartment, and A is the effective area of ​​the membrane.

[0052] On this basis, the cation permeability selectivity P(M) of the membrane was calculated by formula (2) + / D 2+ ):

[0053]

[0054] in, and is the flux of monovalent cations and divalent cations passing through the membrane after the test, and They are the monovalent cations (K + 、Na + or Li + ) and divalent cations (Mg 2+ )’s average concentration.

[0055] The experimental results are shown in Table 1 and Figure 4 shown.

[0056] Table 1

[0057] Performance parameters Comparative Example 1 Example 1 Example 2 <![CDATA[K + / Mg 2+ Optional]]> 147 124 19 <![CDATA[Na + / Mg 2+ Optional]]> 328 325 25 <![CDATA[Li + / Mg 2+ Optional]]> 102 72 14 <![CDATA[K + Mg 2+ Flux (molh -1 m -2 )]]> 0.10、0.00067 0.06、0.00051 0.19、0.0096 <![CDATA[Na + Mg 2+ Flux (molh -1 m -2 )]]> 0.19、0.00058 0.36、0.0011 0.43、0.017 <![CDATA[Li + Mg 2+ Flux (molh -1 m -2 )]]> 0.09、0.00094 0.08、0.0011 0.15、0.010

[0058] By comparison, we can see that:

[0059] The prepared mixed matrix membrane has good + / Mg 2+ ions, and when the addition amount of PCC-67 nanoparticles was 5wt%, it could not only maintain a high Na + / Mg 2+ Selectivity and can increase Na + flux, while reducing K + / Mg 2+ With Li + / Mg 2+ The selectivity and flux of the mixed matrix membrane with 5 wt% PCC-67 nanoparticles can make more Na + It can be used to extract sodium ions from salt lakes, and also to build bionic Na + Ion channels provide one way.

[0060] When the addition amount of PCC-67 nanoparticles is 10wt%, K + 、Na + , Li + The flux increased significantly, and the corresponding Mg 2+ The flux also increased, resulting in a significant decrease in the selectivity of each ion pair. In summary, based on the comprehensive consideration of ion selectivity and flux, when the addition amount of PCC-67 nanoparticles is 5wt%, it is the optimal addition amount.

[0061] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A mixed matrix membrane for ion selective separation, characterized in that: The mixed matrix membrane is prepared by adding PCC-67 nanoparticles as fillers into a quaternized poly(biphenylpiperidine) matrix membrane.

2. A method for preparing the mixed matrix membrane according to claim 1, characterized in that: The steps include: 1) dissolving H3L in a mixture of DMF, ethanol and water to form solution A; dissolving holmium chloride hexahydrate in a mixture of DMF, ethanol and water to form solution B; mixing solution A and solution B, reacting, washing and drying the obtained product to obtain PCC-67 nanoparticles; 2) mixing methyl iodide as a quaternizing agent with poly(biphenyl piperidine) in dimethyl sulfoxide, and performing a room temperature quaternization reaction in the dark to obtain a quaternized poly(biphenyl piperidine); 3) adding PCC-67 nanoparticles and quaternized poly(biphenylpiperidine) into dimethyl sulfoxide and uniformly mixing them by ultrasonication to obtain a membrane solution, and then coating the membrane solution onto a glass plate and drying it to obtain a mixed matrix membrane.

3. The preparation method according to claim 2, characterized in that: In step 1), the molar ratio of H3L to holmium chloride hexahydrate is 1:

3.

4. The preparation method according to claim 2, characterized in that: In step 1), the volume ratio of DMF, ethanol and water is 6:2:0.

5.

5. The preparation method according to claim 2, characterized in that: In step 1), the reaction temperature is 70-80°C and the reaction time is 48-72h.

6. The preparation method according to claim 2, characterized in that: In step 2), the ratio of poly(biphenylpiperidine) to methyl iodide is 1 g:320 μL.

7. The preparation method according to claim 2, characterized in that: In step 3), the mass ratio of PCC-67 nanoparticles to quaternized poly(biphenylpiperidine) is 5-10%:95-90%.

8. The preparation method according to claim 2, characterized in that: In step 3), the drying temperature is 60-80°C.

9. Use of the mixed matrix membrane according to claim 1 as a mono- or polyvalent cation selective ion separation membrane.

Citation Information

Patent Citations

  • Novel metal organic porous cage nanofiltration membrane and preparation method thereof

    CN113069941A

  • POC-based mixed matrix membrane as well as preparation method and application thereof

    CN115869791A

  • Metal-organic cage complex mixed matrix membrane for gas separation as well as preparation method and application of metal-organic cage complex mixed matrix membrane

    CN116059837A