Microporous membrane, ion exchange membrane and application thereof

By introducing hydrophilic ion exchange polymers into the polytetrafluoroethylene microporous membrane and using wet blending technology, the problem of poor structural deformation and compatibility of microporous membranes is solved, and a high-performance ion exchange membrane is realized. In many high-demand applications.

CN118925518APending Publication Date: 2024-11-12FOSHAN LVDONG HYDROGEN ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201583.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polytetrafluoroethylene microporous membranes are structurally deformed when surface modification, which affects the performance of the ion exchange membrane. The hydrophilic materials have poor compatibility with polytetrafluoroethylene particles, resulting in insufficient mechanical properties and conductivity.

Method used

The hydrophilic ion exchange polymer is introduced and blended with polytetrafluoroethylene emulsion, and mixed uniformly by wet preparation method to form a microporous membrane to improve hydrophilicity and mechanical properties, and to form a high-strength fiber structure through bidirectional tensile .

Benefits of technology

It significantly improves the hydrophilicity, mechanical properties and electrical conductivity of the microporous membrane, enhances the filling and durability of the ion exchange membrane, and is suitable for fuel cells and other high-performance applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925518A_ABST
    Figure CN118925518A_ABST
Patent Text Reader

Abstract

The invention discloses a microporous membrane, an ion exchange membrane and application thereof, the microporous membrane comprises polytetrafluoroethylene and a hydrophilic ion exchange polymer, and the hydrophilic ion exchange polymer comprises at least one of a hydrophilic anion exchange polymer and a hydrophilic cation exchange polymer. The hydrophilic ion exchange polymer is introduced into the microporous membrane, so that the hydrophilicity of the e-PTFE can be improved, the filling property of ion exchange resin in the e-PTFE can be improved, and the electrochemical performance, the mechanical performance, the barrier property and the durability can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a microporous membrane, an ion exchange membrane and applications thereof. Background Art

[0002] Polytetrafluoroethylene microporous membrane, referred to as e-PTFE, is a thin film with countless through holes with a pore size between 5nm and 1mm. It is a preferred material in the fields of environmental filtration, clothing, construction, aerospace, ion exchange membrane, etc. At present, the more commonly used ion exchange membrane reinforcement layer is e-PTFE membrane, which has the advantages of high mechanical strength and good chemical stability. However, its hydrophobicity is not conducive to the composite effect of ion exchange resin, and the ionic insulation of the e-PTFE membrane itself limits the further improvement of the conductivity of the ion exchange membrane. An important improvement direction for e-PTFE applied to the reinforcement layer of the ion exchange membrane is to improve the hydrophilicity of e-PTFE. In the related art, the method of hydrophilic modification is to modify the surface of the formed e-PTFE and coat the hydrophilic material on the surface of the e-PTFE by coating. However, the hydrophilic material will cause the structural deformation of the e-PTFE during the coating process, especially the size shrinkage in the thickness direction and the change of the pore size distribution. This structural deformation is not conducive to the preparation of high-performance ion exchange membranes using e-PTFE as a reinforcement layer. Summary of the invention

[0003] The present invention is based on the inventor's discovery and understanding of the following facts and problems: coating a hydrophilic material on the surface of e-PTFE for surface modification will cause deformation of the microporous structure, affecting subsequent applications.

[0004] Another method of hydrophilic modification of microporous membranes is to directly mix hydrophilic materials with polytetrafluoroethylene solid particles, and then process the mixture to obtain e-PTFE. This solid mixing method has simple steps, but the mixing effect is poor. The polarity of hydrophilic materials and polytetrafluoroethylene particles is quite different, and the compatibility is poor. The particle size of polytetrafluoroethylene solid particles generally exceeds 100μm, and the distribution uniformity of the two materials is poor, and the mechanical properties are poor. In addition, hydrophilic materials are introduced into the e-PTFE membrane for modification, but the selected hydrophilic materials do not have ion transmission capabilities, and the modified microporous membrane is still an ion insulator. The e-PTFE prepared by mixing hydrophilic materials with polytetrafluoroethylene particles has the disadvantages of uneven raw material mixing, poor finished product uniformity, low mechanical strength and insulation.

[0005] Fiber materials containing ion exchange polymers have certain ion transmission capabilities. However, they are mainly prepared by electrospinning and solution blowing, which are costly and difficult to mass produce.

[0006] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the embodiments of the present invention provide a microporous membrane, an ion exchange membrane and applications thereof, wherein the introduction of a hydrophilic ion exchange polymer can improve the hydrophilicity of e-PTFE, which is beneficial to improving the filling property of the ion exchange resin in the e-PTFE, and can improve the electrochemical properties, mechanical properties, barrier properties and durability of the ion exchange membrane.

[0007] The embodiment of the present invention provides a microporous membrane, comprising polytetrafluoroethylene and a hydrophilic ion exchange polymer, wherein the hydrophilic ion exchange polymer comprises at least one of a hydrophilic anion exchange polymer or a hydrophilic cation exchange polymer.

[0008] Advantages and technical effects of the microporous membrane of the embodiment of the present invention: the introduction of hydrophilic ion exchange polymer can improve the hydrophilicity of e-PTFE and enable the microporous membrane to have a certain ion exchange capacity and ion transmission capacity. When the microporous membrane is applied to the ion exchange membrane, it is beneficial to improve the filling property of the ion exchange resin in the e-PTFE and enhance the electrochemical performance, mechanical performance, barrier property and durability of the ion exchange membrane.

[0009] In the embodiment of the present invention, the hydrophilic ion exchange polymer can give the insulating e-PTFE microporous membrane a certain ion transmission capacity while improving the hydrophilicity of the microporous membrane fiber, thereby improving the electrochemical properties of the microporous membrane. When the microporous membrane is applied to the ion exchange membrane, the mechanical strength of the ion exchange membrane mainly depends on the fiber structure of the microporous membrane. Relatively speaking, the mechanical strength of the ion exchange resin as the matrix material contributes less to the strength of the ion exchange membrane. The microporous membrane includes polytetrafluoroethylene and hydrophilic ion exchange polymers. The good fibrillation ability of polytetrafluoroethylene is the basis for the stretching and forming of microporous membrane fibers. The high strength of polytetrafluoroethylene makes the microporous membrane fibers and nodes have the characteristics of high strength and high modulus. The fiber structure after compounding with the hydrophilic ion exchange polymer can significantly improve the mechanical properties of the microporous membrane. In addition, when the microporous membrane contains a basic group, it can form ionic crosslinks with the acidic groups in the ion exchange resin, which can improve the combination of the ion exchange resin and the fiber structure in the ion exchange membrane, and significantly enhance the mechanical properties and barrier properties of the ion exchange membrane. However, the molding quality of the blended non-microporous membrane obtained by mixing the hydrophilic ion exchange polymer with PTFE is poor. The two polymers are stacked together in particles / blocks, and the strength improvement effect is much lower than that of the microporous membrane introduced with the fiber structure.

[0010] In some embodiments, the hydrophilic anion exchange polymer comprises a perfluoroazonium ion resin;

[0011] and / or, the hydrophilic cation exchange polymer comprises at least one of a sulfonated polymer, a perfluorosulfonyl imide resin or a phosphonated polymer;

[0012] And / or, the mass ratio of the polytetrafluoroethylene to the hydrophilic ion exchange polymer is 100:0.01-25.

[0013] In some embodiments, the average pore size of the microporous membrane is 0.01 to 1 μm;

[0014] and / or, the porosity of the microporous membrane is 30 to 95%;

[0015] And / or, the microporous membrane has a thickness of 1 to 1000 μm.

[0016] The present invention provides a method for preparing a microporous membrane, comprising the following steps:

[0017] (1) blending a polytetrafluoroethylene emulsion and a hydrophilic ion exchange polymer to obtain a composite;

[0018] (2) Forming the composite into a film to obtain a microporous membrane.

[0019] In the embodiment of the present invention, a hydrophilic ion exchange polymer is added to a polytetrafluoroethylene emulsion to form a dispersion, which is then uniformly mixed with the polytetrafluoroethylene emulsion to prepare a composite, and the composite is then prepared into a microporous membrane, and the hydrophilicity of the hydrophilic ion exchange polymer is used to improve the hydrophilicity of the surface of the microporous membrane. Compared with the solid dry-mixing polymer, the hydrophilic ion exchange polymer is wet-mixed with the polytetrafluoroethylene emulsion to prepare the composite, and the hydrophilic ion exchange polymer is dispersed and mixed with the emulsion more uniformly, and the hydrophilic ion exchange polymer can be uniformly dispersed in the polytetrafluoroethylene, thereby improving the hydrophilicity of the microporous membrane. This is because the average particle size of the polytetrafluoroethylene emulsion is generally 0.1 to 0.5 μm, and the polytetrafluoroethylene solid particles obtained after the emulsion is dried are large particles produced by the emulsion particles as primary particles through the aggregation effect, and the particle size is usually above 100 μm; while in the wet mixed composite, the primary particle size becomes smaller, and the primary particles are formed by the accumulation of emulsion particles and hydrophilic ion exchange polymer solution particles. The hydrophilic ion exchange polymer solution particle size is smaller than the emulsion particle size, and the particle size forming the interface of the hydrophilic ion exchange polymer and polytetrafluoroethylene is smaller, and the mixing uniformity is significantly improved. The e-PTFE obtained by further processing the uniformly mixed hydrophilic ion exchange polymer and polytetrafluoroethylene composite has better mechanical properties and uniformity. The method of the present invention is simple to operate and convenient for scale-up preparation.

[0020] In some embodiments, in step (1), the mass percentage concentration of the polytetrafluoroethylene emulsion is 5% to 90%;

[0021] And / or, in the step (1), the hydrophilic ion exchange polymer and the polytetrafluoroethylene emulsion are uniformly mixed, and then co-coagulated and / or dried to obtain a composite;

[0022] And / or, in step (1), the particle size of the composite is ≤4 mm.

[0023] In some embodiments, in the step (2), the film is formed by biaxial stretching; the biaxial stretching includes MD direction stretching and TD direction stretching, the MD direction stretching multiple is 2 to 15; the TD direction stretching multiple is 2 to 45.

[0024] An embodiment of the present invention provides an ion exchange membrane, comprising an ion exchange resin and a microporous membrane. The microporous membrane is the microporous membrane described in the embodiment of the present invention or a microporous membrane prepared by the preparation method described.

[0025] In the embodiment of the present invention, the hydrophilicity of the microporous membrane of the ion exchange membrane is more conducive to the filling of the ion exchange resin, and the microporous membrane has ion transmission capacity and high mechanical properties, which enhances the mechanical properties, barrier properties, electrochemical properties and durability of the ion exchange membrane. The ion exchange membrane has good durability when applied to the fields of fuel cell ion exchange membrane, ion exchange membrane for hydrogen production by electrolysis of water and flow battery diaphragm. The ion exchange membrane can also be applied to the fields of chlor-alkali industrial diaphragm, electrodialysis membrane and osmotic membrane, and has a wide range of applications.

[0026] In some embodiments, the thickness of the ion exchange membrane is 3 μm to 500 μm;

[0027] And / or, the ion exchange capacity of the ion exchange membrane is 0.1 mmol / g to 5.2 mmol / g.

[0028] The present invention provides a method for preparing an ion exchange membrane, comprising the following steps:

[0029] 1) dispersing an ion exchange resin in a solvent to obtain an ion exchange resin dispersion;

[0030] 2) coating the ion exchange resin dispersion on one side or both sides of a microporous membrane and drying the membrane to obtain an ion exchange membrane.

[0031] The embodiment of the present invention provides an application of a microporous membrane or an ion exchange membrane for at least one of filtration, separation, sealing material, and textile material. In the embodiment of the present invention, all the advantages of the microporous membrane or ion exchange membrane are possessed, which will not be repeated here. The microporous membrane or ion exchange membrane can be applied to some application fields with special requirements such as filtration, separation, sealing, and textile, in particular, in the fields of fuel cells, water electrolysis hydrogen production, and flow batteries.

[0032] In some embodiments, the invention is used in at least one of fuel cells, water electrolysis, flow batteries, chlor-alkali industry, electrodialysis, or osmosis. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 These are contact angle images of e-PTFE-2, e-PTFE-4, De-PTFE-2, and De-PTFE-4.

[0034] Figure 2 are surface SEM images of e-PTFE-2, De-PTFE-2, and De-PTFE-3.

[0035] Figure 3 are cross-sectional SEM images of PEM-2 and D-PEM-2.

[0036] Figure 4 are the polarization curves of PEM-2 and D-PEM-2. DETAILED DESCRIPTION

[0037] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0038] A microporous membrane according to an embodiment of the present invention comprises polytetrafluoroethylene and a hydrophilic ion exchange polymer, wherein the hydrophilic ion exchange polymer comprises at least one of a hydrophilic anion exchange polymer or a hydrophilic cation exchange polymer.

[0039] The microporous membrane of the embodiment of the present invention introduces a hydrophilic ion exchange polymer, which can improve the hydrophilicity of e-PTFE and enable the microporous membrane to have a certain ion exchange capacity and ion transmission capacity. When the microporous membrane is applied to the ion exchange membrane, it is beneficial to improve the filling property of the ion exchange resin in the e-PTFE, and enhance the electrochemical performance, mechanical performance, barrier property and durability of the ion exchange membrane.

[0040] In the embodiment of the present invention, the hydrophilic ion exchange polymer can give the insulating e-PTFE microporous membrane a certain ion transmission capacity while improving the hydrophilicity of the microporous membrane fiber, thereby improving the electrochemical properties of the microporous membrane. When the microporous membrane is applied to the ion exchange membrane, the mechanical strength of the ion exchange membrane mainly depends on the fiber structure of the microporous membrane. Relatively speaking, the mechanical strength of the ion exchange resin as the matrix material contributes less to the strength of the ion exchange membrane. The microporous membrane includes polytetrafluoroethylene and hydrophilic ion exchange polymers. The good fibrillation ability of polytetrafluoroethylene is the basis for the stretching and forming of microporous membrane fibers. The high strength of polytetrafluoroethylene makes the microporous membrane fibers and nodes have the characteristics of high strength and high modulus. The fiber structure after compounding with the hydrophilic ion exchange polymer can significantly improve the mechanical properties of the microporous membrane. In addition, when the microporous membrane contains a basic group, it can form ionic crosslinks with the acidic groups in the ion exchange resin, which can improve the combination of the ion exchange resin and the fiber structure in the ion exchange membrane, and significantly enhance the mechanical properties and barrier properties of the ion exchange membrane. However, the molding quality of the blended non-microporous membrane obtained by mixing the hydrophilic ion exchange polymer with PTFE is poor. The two polymers are stacked together in particles / blocks, and the strength improvement effect is much lower than that of the microporous membrane introduced with the fiber structure.

[0041] In some embodiments, the hydrophilic ion exchange polymer includes at least one of a hydrophilic anion exchange polymer or a hydrophilic cation exchange polymer;

[0042] Optionally, the hydrophilic anion exchange polymer comprises a perfluoronitrogenium ion resin; Optionally, the perfluoronitrogenium ion resin comprises at least one of a quaternary ammonium functionalized perfluororesin, a piperidine functionalized perfluororesin, an imidazole functionalized perfluororesin, a pyridine functionalized perfluororesin, and a pyrrole functionalized perfluororesin;

[0043] Optionally, the hydrophilic cation exchange polymer comprises at least one of a sulfonated polymer, a perfluorosulfonyl imide resin, or a phosphonated polymer;

[0044] Optionally, the sulfonated polymer includes at least one of perfluorosulfonic acid resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, sulfonated polyaryletherketone, sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole;

[0045] Optionally, the phosphonated polymer comprises a perfluorophosphonic acid resin;

[0046] Preferably, the hydrophilic cation exchange polymer includes at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polyetheretherketone, sulfonated polyaryletherketone, and sulfonated polyarylethernitrile; more preferably, the hydrophilic cation exchange polymer includes at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin, and polyacid side chain perfluoro resin.

[0047] In the embodiments of the present invention, the hydrophilic ion exchange polymer can improve the hydrophilicity of the fiber while giving the microporous membrane a certain ion transmission ability. When applied to the ion exchange membrane reinforcement layer, it can reduce the impedance of the reinforcement layer area, reduce local disconnection caused by insulating materials and / or void structures, and enhance the continuity of ion transmission on both sides of the membrane.

[0048] Hydrophilic anion exchange polymers contain basic groups, for example, quaternary ammonium ion groups, imidazolium ion groups, pyridinium ion groups, piperidinium ion groups, pyrrolium ion groups and other nitrogen onium ion groups. The basic groups can form acid-base crosslinks with the acidic groups of the ion exchange resin. This strong physical crosslinking effect can make the ion exchange resin fit more closely to the surface of the microporous membrane fiber, avoiding a large number of void structures or stratification due to poor compatibility, strengthening the continuity of the distribution of the ion exchange resin in the composite ion exchange membrane, and improving the mechanical stability of the ion exchange membrane under complex temperature and humidity conditions.

[0049] Hydrophilic cation exchange polymers include sulfonated polymers or phosphonated polymers, which can increase the surface energy of microporous membranes and have the ability to exchange and transport cations. After being compounded with ion exchange resins to prepare ion exchange membranes, they can improve the filling effect of ion exchange resins in microporous membranes and cooperate with ion exchange resins to carry out ion transport and / or ion exchange. When the ion exchange membrane is a proton exchange membrane, the microporous membrane has a certain proton compensation effect. Improving the hydrophilicity of the microporous membrane can also improve the water retention of the proton exchange membrane, thereby widening the working temperature of the proton exchange membrane.

[0050] The ion exchange groups of hydrophilic ion exchange polymers also have certain antibacterial properties and can play a special role in the field of medical textile materials and water / air filtration.

[0051] In some embodiments, the general structural formula of the perfluorosulfonic acid resin is:

[0052]

[0053] The general structural formula of the polyacid side chain type perfluororesin is:

[0054]

[0055] The general structural formula of the perfluorosulfonyl imide resin is:

[0056]

[0057] The general structural formula of the perfluoronitrogenium ion resin is:

[0058]

[0059] Wherein, a=0-6, b=2-5, c=1-5, d=0-5, e=0-1, a, b, c, d, e are all integers; M is the combined cation, R 1 Selected from C 1 ~C 20 Alkyl; R 2 Selected from C 1 ~C 20 An alkyl group; Q is a nitrogen onium ion group;

[0060] Optionally, the nitrogen onium ion group is selected from at least one of the following structural formulas:

[0061]

[0062] Among them, R 3 ~R 25 Each independently selected from H, C 1 ~C 20 Alkyl or C 6 ~C 20 Aryl, X - Selected from OH - Or halide ion; Optionally, the halide ion is selected from at least one of fluoride ion, chloride ion, bromide ion and iodide ion;

[0063] Optionally, perfluorosulfonic acid resin, polyacid side chain perfluoro resin, perfluorosulfonyl imide resin and perfluoronitrogenium ion resin can all be obtained by substitution reaction using sulfonyl fluoride resin as raw material; these resins are all composed of tetrafluoroethylene repeating units and perfluorovinyl ether derivative repeating units, and the difference lies in the end group structure of the perfluorovinyl ether derivative; when the perfluorovinyl ether derivative repeating unit structure is determined, the ion exchange equivalent (EW) of the resin is determined by x, and the value of EW is the molecular weight of the tetrafluoroethylene repeating unit multiplied by x plus the molecular weight of the perfluorovinyl ether derivative repeating unit; y determines the molecular weight of the material.

[0064] In some embodiments, the EW of the hydrophilic ion exchange polymer is 400-5000 g / mol, preferably 500-2000 g / mol, more preferably 600-1200 g / mol; the number average molecular weight (Mn) of the hydrophilic ion exchange polymer is 50000-3000000, preferably 60000-1500000, more preferably 70000-800000l.

[0065] In the embodiments of the present invention, the appropriate EW value and molecular weight are conducive to further improving the hydrophilicity and mechanical properties of the material. If the EW is too low, the hydrophilicity of the material is too strong, and it is very easy to dissolve during the processing and use of the microporous membrane, resulting in quality loss. If the EW is too high, the hydrophilicity is reduced, the dissolution processing is difficult, and the effect of improving the hydrophilicity of the microporous membrane material is limited. The stability and mechanical properties of the material with too low molecular weight are low, and it is difficult to process and shape; the material with high molecular weight is difficult to prepare and difficult to dissolve.

[0066] In some embodiments, the hydrophilic cation exchange polymer can bind different cations (M), optionally, the cation includes at least one of hydrogen ions, ammonium ions, and metal ions; the metal ions include at least one of monovalent metal cations, alkaline earth metal ions or other multivalent cations; specifically, the metal ions include at least one of lithium ions, sodium ions, potassium ions, silver ions, magnesium ions, calcium ions, copper ions, iron ions, zirconium ions, cerium ions, manganese ions, aluminum ions, titanium ions, vanadium ions or zinc ions.

[0067] In some embodiments, the mass ratio of the polytetrafluoroethylene to the hydrophilic ion exchange polymer is 100:0.01-25, specifically, for example, 100:0.01, 100:0.1, 100:0.2, 100:0.5, 100:1, 100:1.5, 100:2, 100:5, 100:10, 100:20, 100:25, preferably, 100:0.1-10, further preferably, 100:0.1-5, more preferably, 100:0.1-2. In the embodiment of the present invention, by adjusting the content of the hydrophilic ion exchange polymer, it is beneficial for the microporous membrane to maintain good mechanical properties while improving the hydrophilicity. Too low a content of the hydrophilic ion exchange polymer will result in insufficient hydrophilicity of the microporous membrane, and too high a content may not be easy to mix evenly and the mechanical properties of the obtained e-PTFE may be poor.

[0068] In some embodiments, the average pore size of the microporous membrane is 0.01 to 1 μm, preferably 0.03 to 0.7 μm, and more preferably 0.05 to 0.5 μm.

[0069] In some embodiments, the porosity of the microporous membrane is 30-95%, preferably 40-90%, and more preferably 60-90%.

[0070] In some embodiments, the microporous membrane has a thickness of 1 to 1000 μm, preferably 2 to 300 μm, further preferably 3 to 100 μm, and more preferably 3 to 50 μm.

[0071] In some embodiments, the microporous membrane is a fiber structure; optionally, the microporous membrane is prepared by biaxial stretching.

[0072] A method for preparing a microporous membrane according to an embodiment of the present invention comprises the following steps:

[0073] (1) blending a polytetrafluoroethylene emulsion and a hydrophilic ion exchange polymer to obtain a composite;

[0074] (2) Forming the composite into a film to obtain a microporous membrane.

[0075] In the embodiment of the present invention, a hydrophilic ion exchange polymer is added to a polytetrafluoroethylene emulsion to form a dispersion, which is then uniformly mixed with the polytetrafluoroethylene emulsion to prepare a composite, and the composite is then prepared into a microporous membrane, and the hydrophilicity of the hydrophilic ion exchange polymer is used to improve the hydrophilicity of the surface of the microporous membrane. Compared with the solid dry-mixing polymer, the hydrophilic ion exchange polymer is wet-mixed with the polytetrafluoroethylene emulsion to prepare the composite, and the hydrophilic ion exchange polymer is dispersed and mixed with the emulsion more uniformly, and the hydrophilic ion exchange polymer can be uniformly dispersed in the polytetrafluoroethylene, thereby improving the hydrophilicity of the microporous membrane. This is because the average particle size of the polytetrafluoroethylene emulsion is generally 0.1 to 0.5 μm, and the polytetrafluoroethylene solid particles obtained after the emulsion is dried are large particles produced by the emulsion particles as primary particles through the aggregation effect, and the particle size is usually above 100 μm; while in the wet mixed composite, the primary particle size becomes smaller, and the primary particles are formed by the accumulation of emulsion particles and hydrophilic ion exchange polymer solution particles. The hydrophilic ion exchange polymer solution particle size is smaller than the emulsion particle size, and the particle size forming the interface of the hydrophilic ion exchange polymer and polytetrafluoroethylene is smaller, and the mixing uniformity is significantly improved. The e-PTFE obtained by further processing the uniformly mixed hydrophilic ion exchange polymer and polytetrafluoroethylene composite has better mechanical properties and uniformity. The method of the present invention is simple to operate and convenient for scale-up preparation.

[0076] In some embodiments, in the step (1), the polytetrafluoroethylene emulsion comprises polytetrafluoroethylene and water. Preferably, the mass percentage concentration (solid content) of the polytetrafluoroethylene emulsion is 5% to 90%, specifically, for example, 5%, 10%, 20%, 25%, 30%, 45%, 50%, 60%, 70%, 80%, 90%, further preferably, 25% to 80%, more preferably, 30% to 70%. In the embodiment of the present invention, the polytetrafluoroethylene resin raw material is a polytetrafluoroethylene emulsion obtained by emulsion polymerization. The average particle size of the polytetrafluoroethylene emulsion is mainly distributed in the range of 0.1 to 0.5 μm, generally not less than 0.01 μm and not more than 1 μm. Such small particle size particles are also called primary particles. Polytetrafluoroethylene emulsions of different concentrations can be blended with hydrophilic ion exchange polymers to form a composite. When the concentration of polytetrafluoroethylene is low, the drying efficiency is relatively low. When the concentration is high, it may cause difficulty in dispersing the hydrophilic ion exchange polymer dispersion in the emulsion.

[0077] In some embodiments, in step (1), the hydrophilic ion exchange polymer is a hydrophilic ion exchange polymer dispersion and / or a hydrophilic ion exchange polymer solid. In the embodiment of the present invention, since the hydrophilic ion exchange polymer solid dissolves and disperses slowly in the polytetrafluoroethylene emulsion, in order to improve the mixing efficiency, the polytetrafluoroethylene emulsion and the hydrophilic ion exchange polymer dispersion are preferably blended to obtain a composite for a microporous membrane.

[0078] In some embodiments, a hydrophilic ion exchange polymer is dispersed in a solvent to obtain a hydrophilic ion exchange polymer dispersion; optionally, the solvent includes at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, tetramethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, water, methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol; preferably, the solvent includes at least one of tetrahydrofuran, water, methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol; more preferably, the solvent includes at least one of water, ethanol, n-propanol, and isopropanol. In the embodiments of the present invention, a solvent with a low boiling point, low toxicity, and low pollution is preferred, which has a good effect of dispersing the hydrophilic ion exchange polymer and has good miscibility with water in the polytetrafluoroethylene emulsion.

[0079] In some embodiments, the mass percentage concentration of the hydrophilic ion exchange polymer dispersion is 0.1% to 60%, specifically, for example, 0.1%, 1%, 4%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, preferably, 1% to 50%, more preferably, 4% to 40%. In the embodiments of the present invention, the hydrophilic ion exchange polymer has good dispersibility in the water of the polytetrafluoroethylene emulsion, and the concentration of the hydrophilic polymer dispersion has little effect on the mixing process. A low concentration will result in a large volume of the added dispersion, and a high concentration will result in a longer mixing time.

[0080] In some embodiments, in step (1), the blending is performed by wet mixing, including: uniformly mixing the hydrophilic ion exchange polymer and the polytetrafluoroethylene emulsion to obtain a mixed dispersion, and then co-coagulating and / or drying to obtain a composite;

[0081] Optionally, the mixed dispersion is co-coagulated and dried to obtain a composite;

[0082] Optionally, the mixed dispersion is directly dried to obtain a composite;

[0083] Optionally, the co-coagulation may adopt a variety of co-coagulation methods, preferably, a mechanical stirring method;

[0084] Optionally, the drying includes at least one of spray drying, freeze drying, and vacuum drying.

[0085] In some embodiments, the drying temperature is ≤200° C., preferably ≤100° C., and more preferably ≤19° C. In the embodiments of the present invention, during the drying of the composite solid, excessively high drying temperature may cause the polytetrafluoroethylene solid to undergo crystal transformation and severe aggregation effect, resulting in severe agglomeration of the obtained polytetrafluoroethylene solid or large particle size, which is not conducive to subsequent processing and molding of the composite.

[0086] In some embodiments, the composite is a solid particle; optionally, the particle size of the composite is ≤4 mm, preferably ≤2 mm, further preferably ≤1 mm, and more preferably 200-800 μm. In the embodiments of the present invention, a larger particle size of the composite will result in insufficient mixing of polytetrafluoroethylene in the additive oil, and the uniformity of the membrane product will be relatively poor. A smaller particle size will increase the difficulty of the preparation process, which is not conducive to large-scale production.

[0087] In some embodiments, in step (2), the film is formed by biaxial stretching;

[0088] Optionally, the biaxial stretching adopts multiple stretching in TD and / or MD directions;

[0089] Optionally, the biaxial stretching adopts static biaxial stretching;

[0090] Optionally, the biaxial stretching includes first stretching in the MD direction and then stretching in the TD direction;

[0091] Optionally, the biaxial stretching includes first stretching in the TD direction and then stretching in the MD direction;

[0092] Optionally, the biaxial stretching includes first stretching in the TD direction, then stretching in the MD direction, and finally stretching in the TD direction once more;

[0093] Optionally, the biaxial stretching includes stretching in the MD direction and stretching in the TD direction, the stretching multiple in the MD direction is 2 to 15; the stretching multiple in the TD direction is 2 to 45;

[0094] Among them, according to the conventional definition in the field of preparing microporous membranes by stretching method, the direction of mechanical force is MD, and the direction transverse to the mechanical force is TD. In the e-PTFE industry, the MD direction is usually called the longitudinal direction and the TD direction is called the transverse direction.

[0095] In an embodiment of the present invention, a biaxial stretching method is used to prepare a polytetrafluoroethylene microporous membrane on a large scale. During the stretching process, the polytetrafluoroethylene material in the composite first forms a highly oriented structure in one direction, and then forms a mesh structure composed of nodes and fibers in all directions. The polytetrafluoroethylene material itself has the characteristics of high strength and high modulus, and the fibers and nodes in the formed fiber mesh structure have excellent mechanical properties. After biaxial stretching, the fibers are centered on the nodes and radially form a mesh structure, so that the microporous membrane has a large number of through holes and has good dimensional stability and mechanical properties. The through-hole structure can meet its application requirements as a filter material, a waterproof and breathable material, and a composite material reinforcement layer, and its good mechanical strength enables it to effectively enhance the mechanical strength of the composite membrane material.

[0096] In some embodiments, the film forming comprises the following steps:

[0097] 1) mixing the composite material and the auxiliary oil, performing aging, blanking, extrusion and calendering to obtain a calendered belt or calendered film;

[0098] Optionally, the auxiliary oil includes at least one of gasoline and kerosene; the mass ratio of the composite to the auxiliary oil is 100:10-50;

[0099] Optionally, the aging is to place the mixture of the composite and the auxiliary oil at a certain temperature for a certain period of time; the aging temperature is 20 to 100° C., and the aging time is 1 hour to 1 week;

[0100] Optionally, the blanking is to extrude the matured mixture into a blank in a mold; the blanking pressure is 1 to 10 MPa, and the blanking flow rate is 5% to 50%;

[0101] Optionally, the extrusion is to extrude the billet into a strip billet; the extrusion pressure is 1-10 MPa, the extrusion flow rate is 5%-20%, and the extrusion temperature is 20-180° C.;

[0102] Optionally, the calendering is to press the strip into a calendered belt or a calendered film; the calendering temperature is 20 to 180° C., and the calendering roller temperature is 20 to 200° C.;

[0103] 2) drying the calendered belt or calendered film to obtain a degreased film; biaxially stretching the degreased film and then heat-setting it to obtain a microporous film;

[0104] Optionally, the biaxial stretching adopts multiple stretching in TD and / or MD directions; Optionally, the biaxial stretching adopts static biaxial stretching; Optionally, the biaxial stretching includes first stretching the degreased film in MD direction and then stretching it in TD direction; Optionally, the biaxial stretching includes first stretching the degreased film in TD direction, then stretching it in MD direction, and finally stretching it in TD direction once; Optionally, the biaxial stretching includes stretching in MD direction and stretching in TD direction, and the multiple of stretching in MD direction is 2 to 15; the multiple of stretching in TD direction is 2 to 45;

[0105] Optionally, the drying temperature is 90 to 300° C., and the drying time is 1 to 120 min;

[0106] Optionally, the heat setting refers to the phase transition of the biaxially stretched microporous membrane at high temperature to form a high-temperature crystal with higher strength and modulus, thereby improving the mechanical strength and dimensional stability of the microporous membrane; the heat setting temperature is 280 to 420°C; and the heat setting time is 1 to 60 minutes.

[0107] Optionally, the microporous membrane is heat-treated after heat setting to improve its mechanical properties; the heat treatment includes at least one of roller heating and electric baking; the temperature of the heat treatment is 350-450°C.

[0108] An ion exchange membrane according to an embodiment of the present invention comprises an ion exchange resin and a microporous membrane. The microporous membrane is the microporous membrane according to the embodiment of the present invention or a microporous membrane prepared by the preparation method according to the embodiment of the present invention.

[0109] In the embodiment of the present invention, the hydrophilicity of the microporous membrane of the ion exchange membrane is more conducive to the filling of the ion exchange resin, and the microporous membrane has ion transmission capacity and high mechanical properties, which enhances the mechanical properties, barrier properties, electrochemical properties and durability of the ion exchange membrane. The ion exchange membrane has good durability when applied to the fields of fuel cell ion exchange membrane, ion exchange membrane for hydrogen production by electrolysis of water and flow battery diaphragm. The ion exchange membrane can also be applied to the fields of chlor-alkali industrial diaphragm, electrodialysis membrane and osmotic membrane, and has a wide range of applications.

[0110] In some embodiments, the ion exchange resin is loaded on one side or both sides of the microporous membrane, that is, the ion exchange resin is arranged on one side or both sides of the microporous membrane along the thickness direction thereof.

[0111] In some embodiments, the thickness of the ion exchange membrane is 3 μm to 500 μm, preferably 4 μm to 320 μm, and more preferably 5 μm to 100 μm.

[0112] In some embodiments, the ion exchange capacity of the ion exchange membrane is 0.1 mmol / g to 5.2 mmol / g, preferably, 0.15 mmol / g to 3.0 mmol / g, and more preferably, 0.2 mmol / g to 2 mmol / g.

[0113] In some embodiments, the ion exchange resin comprises at least one of a hydrophilic anion exchange polymer or a hydrophilic cation exchange polymer; optionally, the hydrophilic anion exchange polymer comprises a perfluoroazonium ion resin; optionally, the hydrophilic cation exchange polymer comprises at least one of a sulfonated polymer or a phosphonated polymer; preferably, the sulfonated polymer comprises a perfluorosulfonic acid resin, a perfluorosulfonimide resin, a polyacid side chain perfluoro resin, a sulfonated polytrifluorostyrene, a sulfonated polysulfone, a sulfonated polyethersulfone, a sulfonated polyetheretherketone, a sulfonated polyaryletherketone, At least one of sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole; further preferably, the sulfonated polymer includes at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polyetheretherketone, sulfonated polyaryletherketone and sulfonated polyarylethernitrile; more preferably, the sulfonated polymer includes at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin and polyacid side chain perfluoro resin; the phosphonated polymer includes perfluorophosphonic acid resin. The general structural formulas of perfluorosulfonic acid resin, polyacid side chain perfluoro resin, perfluorosulfonimide resin and perfluoronitrogenium ion resin are shown in formulas (1) to (4).

[0114] In some embodiments, the hydrophilic cation exchange polymer can bind different cations. Optionally, the cation includes at least one of hydrogen ions, ammonium ions, and metal ions; the metal ions include at least one of monovalent metal cations, alkaline earth metal ions, or other multivalent cations; specifically, the metal ions include at least one of lithium ions, sodium ions, potassium ions, silver ions, magnesium ions, calcium ions, copper ions, iron ions, zirconium ions, cerium ions, manganese ions, aluminum ions, titanium ions, vanadium ions, or zinc ions.

[0115] In some embodiments, the EW of the ion exchange resin is 400-5000 g / mol, preferably 500-2000 g / mol, more preferably 600-1200 g / mol; the number average molecular weight (Mn) of the ion exchange resin is 50,000-3,000,000, preferably 60,000-1,500,000, more preferably 70,000-800,000.

[0116] In some embodiments, the ion exchange resin may be the same as or different from the hydrophilic ion exchange polymer in the microporous membrane.

[0117] A method for preparing an ion exchange membrane according to an embodiment of the present invention comprises the following steps:

[0118] 1) dispersing an ion exchange resin in a solvent to obtain an ion exchange resin dispersion;

[0119] 2) coating the ion exchange resin dispersion on one side or both sides of a microporous membrane and drying the membrane to obtain an ion exchange membrane.

[0120] In the embodiment of the present invention, the microporous membrane and the ion exchange resin have good bonding force, the method is simple and easy to operate, and is convenient for application in industrial production.

[0121] In some embodiments, in step 1), the ion exchange resin is dispersed in a solvent to obtain an ion exchange resin dispersion; optionally, the solvent includes at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, tetramethyl sulfoxide, N-methylpyrrolidone, tetrahydrofuran, water, methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol; preferably, the solvent includes at least one of tetrahydrofuran, water, methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol; more preferably, the solvent includes at least one of water, ethanol, n-propanol and isopropanol.

[0122] In some embodiments, in step 1), the mass percentage concentration of the ion exchange resin dispersion is 0.1% to 60%, specifically, for example, 0.1%, 1%, 4%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, preferably, 1% to 50%, further preferably, 4% to 40%.

[0123] In some embodiments, in step 2), the coating comprises at least one of dipping, blade coating, and slit coating.

[0124] In some embodiments, in step 2), the drying temperature is 40 to 200° C.; and / or the drying time is 1 min to 24 h.

[0125] In some embodiments, in the step 2), heat treatment is performed after drying; optionally, the temperature of the heat treatment is 100 to 220° C.; optionally, the time of the heat treatment is 1 to 120 min.

[0126] In the embodiment of the present invention, the drying process is to remove the solvent and regulate the physical structure of the polymer. Heat treatment after drying can further improve the physical structure of the ion exchange membrane. For example, the perfluororesin needs to be heat treated and crystallized above the glass transition temperature. Crystallization can improve the mechanical strength, chemical stability and solvent resistance of the ion exchange membrane.

[0127] The application of a microporous membrane or ion exchange membrane in an embodiment of the present invention is used for at least one of filtration, separation, sealing material, and textile material. In the embodiment of the present invention, all the advantages of the microporous membrane or ion exchange membrane are possessed, which will not be repeated here. The microporous membrane or ion exchange membrane can be applied to some application fields with special requirements such as filtration, separation, sealing, and textile, in particular, in the fields of fuel cells, water electrolysis hydrogen production, and liquid flow batteries.

[0128] In some embodiments, it is used for at least one of fuel cells, water electrolysis, liquid flow batteries, chlor-alkali industry, electrodialysis or osmosis; preferably, it is used for fuel cell ion exchange membranes, ion exchange membranes for water electrolysis to produce hydrogen, liquid flow battery diaphragms, chlor-alkali industry diaphragms, electrodialysis membranes or osmosis membranes.

[0129] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0130] The perfluorosulfonic acid resin or dispersion used in the embodiments of the present invention is from Chemours, 3M and Solvay. The polyacid side chain type perfluororesin is from 3M. The perfluorosulfonyl imide resin is homemade and is obtained by copolymerizing tetrafluoroethylene and perfluorosulfonyl imide vinyl ether monomers.

[0131] e-PTFE pore size test: The test method is the bubble pressure method (gas-liquid displacement technology), and the test instrument is the Porometer3G pore size analyzer. The wet-first-dry mode is adopted, that is, the e-PTFE is fully wetted with a liquid that can be infiltrated with it, and then a pressure difference is applied to both sides of the membrane to overcome the surface tension of the infiltrating liquid in the membrane pores, and the infiltrating liquid is driven through the pores to obtain the pore size distribution of the e-PTFE. The gas source is compressed air and nitrogen, and the test area is 3.14cm 2 . Take 3 to 5 groups of samples for parallel experiments each time.

[0132] e-PTFE porosity test: The test equipment is a 0.0001g high-precision balance and a true density analyzer; cut three square membranes of the same specifications and sizes without wrinkles, defects and damage as test samples. Use an analytical balance to weigh the mass of the three samples. Calculate the bulk density according to the following formula (1) as the apparent density of the sample:

[0133]

[0134] Where:

[0135] ρ—Volume density of the sample, in grams per cubic centimeter (g / cm 3 );

[0136] m—the mass measurement of the sample, in grams (g);

[0137] d—measured value of the thickness of the sample, in micrometers (μm);

[0138] S—sampling area of ​​the sample, fixed as the sampling knife area, its value is 25cm 2 ;

[0139] The porosity is calculated according to the following formula (2):

[0140]

[0141] Where:

[0142] P—porosity of the sample, dimensionless physical quantity (%);

[0143] ρ—apparent density of the sample, which is the calculated value of the test, in grams per cubic centimeter (g / cm 3 );

[0144] ρ 0 —True density of the sample, in grams per cubic centimeter (g / cm 3 ), obtained by testing with a true density analyzer.

[0145] Contact angle test: The sessile drop method is used, the droplet is water, and the solid sample is e-PTFE. The contact angle between the droplet and the microporous membrane is measured at 16 seconds. The smaller the contact angle, the better the hydrophilicity.

[0146] e-PTFE membrane thickness test: The test equipment is a contact flat-head thickness gauge. Use a cutter to cut three microporous membrane sheets as test specimens. When measuring the thickness, take points equidistantly along the MD (longitudinal) and TD (transverse) directions of the specimen for matrix testing, and calculate the average value of each point as the average thickness of the membrane.

[0147] Free radical resistance: The ion exchange membrane was immersed in Fenton's reagent at 80°C for 8 h, and the mass loss before and after different immersion times was compared. 2 O 2 0.1 mL of Fe with a molar concentration of 0.01 mol / L was added to the solution. 2+ The solution is the Fenton reagent, which is prepared and used immediately. The smaller the mass loss percentage, the better the durability.

[0148] The test methods for conductivity, EW, IEC and tensile strength refer to GB / T20042.3-2022 "Proton Exchange Membrane Fuel Cell Part 3: Proton Exchange Membrane Test Methods". The test conditions for conductivity are 80°C and 95% relative humidity.

[0149] Fuel cell polarization curve and hydrogen permeation current: The test method refers to GB / T20042.5-2022 "Proton Exchange Membrane Fuel Cell Part 5: Membrane Electrode Test Method", and the test conditions are 80°C and 90% relative humidity. The polarization curve reflects the performance of a single cell, and the smaller the hydrogen permeation current, the better the barrier property of the ion exchange membrane.

[0150] Gas barrier properties: Oxygen permeability test and calculation method are carried out according to national standard GB1038-2000.

[0151] Example 1

[0152] 0.1 parts of PFIA resin were added to 250 parts (15 kg) of polytetrafluoroethylene emulsion (solid content 40%, including 100 parts of polytetrafluoroethylene) and stirred and mixed. During the stirring process, PFIA was dissolved in water to form a dispersion. After sufficient mixing, it was spray-dried at room temperature to obtain a composite PTFE-1.

[0153] PFIA resin is a polyacid side chain perfluorinated resin. The EW of PFIA resin is 625 g / mol, and the structural formula is:

[0154]

[0155] Example 2

[0156] 2 parts and 20 parts of sodium-type Aquivion resin dispersion (the mass content of sodium-type Aquivion resin is 28%, and the solvent is water) were added to 10 kg of polytetrafluoroethylene emulsion (solid content 60%, containing 100 parts of polytetrafluoroethylene), respectively, and the mixture was stirred and mixed. After sufficient mixing, the mixture was freeze-dried to obtain composites PTFE-2 and PTFE-3.

[0157] The preparation method of the sodium-type Aquivion resin dispersion is to add about 0.417 parts of NaOH to 30 parts of the acid-type Aquivion resin dispersion (the mass content of the acid-type Aquivion resin is 25%, and the solvent is water) to make the dispersion neutral, and obtain the sodium-type Aquivion resin dispersion after mixing, in which the cations bound to the sulfonic acid groups of the perfluorosulfonic acid resin in the dispersion are sodium ions.

[0158] The EW value of acid-type Aquivion resin is 720 g / mol, and the structural formula is:

[0159]

[0160] Example 3

[0161] To 10 kg of polytetrafluoroethylene emulsion (solid content 60%, including 100 parts of polytetrafluoroethylene), add 20 parts of Nafion resin dispersion (the mass content of Nafion resin is 5%, and the solvent is water, n-propanol and ethanol), stir and mix, mix thoroughly and co-coagulate, and vacuum dry at 15°C to obtain a composite PTFE-4.

[0162] The EW value of Nafion resin is 980g / mol, and the structural formula is:

[0163]

[0164] Example 4

[0165] To 10 kg of polytetrafluoroethylene emulsion (solid content 60%, including 100 parts of polytetrafluoroethylene), add 20 parts of perfluorosulfonyl imide resin dispersion (the mass content of perfluorosulfonyl imide is 1%, and the solvent is equal volumes of water and isopropanol), stir and mix, mix thoroughly and co-coagulate, and vacuum dry at 15°C to obtain a composite PTFE-5.

[0166] The EW value of perfluorosulfonyl imide resin is 1200 g / mol, and the structural formula is:

[0167]

[0168] Example 5

[0169] 1.9 parts of 3M resin were dispersed in 17.9 parts of water, and then about 0.143 parts of KOH were added to make the dispersion neutral to obtain a potassium-type 3M resin dispersion (resin mass content was 10%). The potassium-type 3M resin dispersion was added to 10 kg of polytetrafluoroethylene emulsion (solid content 60%, containing 100 parts of polytetrafluoroethylene), stirred and mixed, and freeze-dried after sufficient mixing to obtain a composite PTFE-6.

[0170] The EW value of 3M resin is 800g / mol, and the structural formula is:

[0171]

[0172] Example 6

[0173] To 10 kg of polytetrafluoroethylene emulsion (solid content 60%, including 100 parts of polytetrafluoroethylene), add 20 parts of quaternary ammonium functionalized perfluororesin dispersion (resin mass content is 10%, solvent is dimethyl sulfoxide), stir and mix, mix thoroughly and co-coagulate, and vacuum dry at 15°C to obtain a composite PTFE-4QA.

[0174] The IEC of quaternary ammonium functionalized perfluororesin is 1.10mmol / g, and the structural formula is:

[0175]

[0176] Example 7

[0177] The difference from Example 5 is that the hydrophilic ion exchange resin material is a piperidine-functionalized perfluororesin, and other conditions are the same to obtain a composite PTFE-4QB.

[0178] The IEC of piperidine functionalized perfluororesin is 1.10mmol / g, and the structural formula is:

[0179]

[0180] Example 8

[0181] The composite PTFE-1 in Example 1 was sieved to obtain 100 parts by mass of 10-40 mesh pellets, 22.5 parts of Isopar K type auxiliary oil were added and mixed, aged at 60°C for 24h, pressed at 2.5MPa, and pressed and extended at 3MPa and 60°C to prepare a calendering belt containing auxiliary oil. After removing the auxiliary oil at high temperature, a degreased film was obtained, which was a dense PTFE film. The degreased film was pre-stretched 1.2 times in the transverse direction (TD direction), stretched 6.2 times in the longitudinal direction (MD direction), and finally stretched 18 times in the transverse direction (TD direction), and sintered and shaped at 390°C for 5min to obtain a modified PTFE microporous membrane e-PTFE-1.

[0182] Example 9

[0183] The composite PTFE-2 in Example 2 was screened, aged, pressed, and pushed to form a calendered belt containing auxiliary oil. The auxiliary oil was removed at high temperature to obtain a degreased film, which was a dense PTFE film. The preparation method of the degreased film was the same as that of Example 8. The dense PTFE film was stretched 6 times in the longitudinal direction (MD direction) and then stretched 20 times in the transverse direction (TD direction), and sintered at 395°C for 3 minutes to obtain a modified PTFE microporous membrane e-PTFE-2.

[0184] Example 10

[0185] The composite PTFE-3 in Example 2 was processed into a degreased membrane according to the method in Example 9. The degreased membrane was a dense PTFE film. The dense PTFE film degreased membrane was subjected to static biaxial stretching (8 times in MD direction and 60 times in TD direction) to obtain a modified PTFE microporous membrane e-PTFE-3.

[0186] Embodiment 11

[0187] The difference from Example 9 is that the raw material of the microporous membrane is the composite PTFE-4 in Example 3, and the transverse stretching multiple is 10 times to obtain a modified PTFE microporous membrane e-PTFE-4.

[0188] Example 12

[0189] Different from Example 9, the raw material of the microporous membrane is the composite PTFE-5 in Example 4, the longitudinal stretching multiple is 5 times, and the transverse stretching multiple is 10 times, so as to obtain a modified PTFE microporous membrane e-PTFE-5.

[0190] Embodiment 13

[0191] The difference from Example 12 is that the raw material of the microporous membrane is the composite PTFE-6 in Example 5, and the transverse stretching multiple is 6 times to obtain a modified PTFE microporous membrane e-PTFE-6.

[0192] Embodiment 14

[0193] The difference from Example 11 is that the raw material of the microporous membrane is the composite PTFE-4QA in Example 6, and a modified PTFE microporous membrane e-PTFE-4QA is prepared.

[0194] Embodiment 15

[0195] The difference from Example 11 is that the raw material of the microporous membrane is the composite PTFE-4QB in Example 7, and a modified PTFE microporous membrane e-PTFE-4QB is prepared.

[0196] Example 16

[0197] The 3M resin in Example 5 was dissolved and dispersed in a mixed solvent of water and n-propanol (water-to-alcohol mass ratio of 1:2) to obtain a resin dispersion with a solid content of 20%. The resin dispersion was slit coated on both sides of the modified microporous membrane e-PTFE-2, and the ion exchange membrane PEM-2 was obtained after drying.

[0198] Embodiment 17

[0199] The difference from Example 16 is that the ion exchange resin is the PFIA resin in Example 1, and the modified microporous membrane is e-PTFE-3, so as to obtain the ion exchange membrane PEM-3.

[0200] Embodiment 18

[0201] The Nafion resin dispersion in Example 3 was coated on both sides of the e-PTFE-4 by a doctor blade, dried at 80° C. for 15 min, and heat treated at 150° C. for 15 min to obtain an ion exchange membrane PEM-4.

[0202] Embodiment 19

[0203] The perfluorosulfonyl imide resin in Example 4 was dissolved and dispersed in a mixed solvent of water and isopropanol (water-to-alcohol mass ratio of 2:8) to obtain a resin dispersion with a solid content of 10%. The dispersion was coated on both sides of the modified microporous membrane e-PTFE-6 by a doctor blade to obtain an ion exchange membrane PEM-6.

[0204] Embodiment 20

[0205] Different from Example 18, the modified microporous membrane is e-PTFE-4QA, and the ion exchange membrane PEM-4QA is obtained.

[0206] Comparative Example 1

[0207] Different from Example 2, no hydrophilic ion exchange polymer is added to the polytetrafluoroethylene emulsion, and solid polytetrafluoroethylene D-PTFE-2 is obtained by freeze drying.

[0208] Comparative Example 2

[0209] 0.56 parts of the sodium-type Aquivion resin solid in Example 2 were added to 100 parts of D-PTFE-2 in Comparative Example 1, and the two solids were stirred and mixed to obtain a mixture D-PTFE-3. The sodium-type Aquivion resin solid was in powder form with a particle size distribution of 200 to 800 μm.

[0210] Comparative Example 3

[0211] The difference from Example 9 is that the raw material for preparing the microporous membrane is D-PTFE-2 in Comparative Example 1, and the microporous membrane De-PTFE-2 is obtained.

[0212] Comparative Example 4

[0213] Different from Example 9, the raw material for preparing the microporous membrane is D-PTFE-3 in Comparative Example 2, and the microporous membrane De-PTFE-3 is obtained.

[0214] Comparative Example 5

[0215] Different from Example 11, the raw material for preparing the microporous membrane is D-PTFE-2 in Comparative Example 1, and the microporous membrane De-PTFE-4 is obtained.

[0216] Comparative Example 6

[0217] Different from Example 16, the reinforcement layer of the ion exchange membrane is De-PTFE-2 in Comparative Example 3, and the ion exchange membrane D-PEM-2 is obtained.

[0218] Comparative Example 7

[0219] The difference from Example 18 is that the reinforcement layer of the ion exchange membrane is De-PTFE-4 in Comparative Example 4, and the ion exchange membrane D-PEM-4 is obtained.

[0220] Comparative Example 8

[0221] Different from Example 18, no microporous membrane reinforcement layer was used, and the Nafion resin dispersion in Example 3 was directly coated by blade coating, dried at 80°C for 15 minutes, and heat treated at 150°C for 15 minutes to obtain an ion exchange membrane D-PEM-4C with an average thickness of 25 μm. The strengths of D-PEM-4C in the TD and MD directions were 13.4 MPa and 12.9 MPa, respectively.

[0222] Comparative Example 9

[0223] 20 g of the Nafion resin dispersion in Example 3 was added to 100 g of the polytetrafluoroethylene emulsion in Example 3, stirred and mixed, and then coated with a doctor blade for molding after sufficient mixing, dried at 80° C. for 15 min, and heat treated at 150° C. for 15 min to obtain a film D-PEM-4F with an average thickness of 25 μm. The strengths of D-PEM-4F in the TD and MD directions were 21.4 MPa and 18.7 MPa, respectively.

[0224] Comparative Example 10

[0225] 50 g of the polytetrafluoroethylene emulsion in Example 3 was coated with a doctor blade, dried at 80° C. for 15 min, and heat treated at 150° C. for 15 min to obtain a polytetrafluoroethylene film M-PTFE with an average thickness of 25 μm. The strength of M-PTFE in the TD and MD directions was 22.6 MPa and 21.5 MPa, respectively.

[0226] Table 1 shows the thickness, hydrophilic ion exchange polymer content, average pore size and porosity of the modified PTFE microporous membrane.

[0227] Table 1

[0228]

[0229] Table 2 shows the pore size distribution, MD and TD tensile strength of the modified PTFE microporous membrane. The solid material whose skeleton material is PTFE can be prepared into modified microporous membranes with different thicknesses, different pore size distributions and high strength by the stretching method.

[0230] Table 2

[0231]

[0232] Figure 1The contact angle images of e-PTFE-2, e-PTFE-4, De-PTFE-2, and De-PTFE-4. The microporous membranes with similar preparation methods, thickness, porosity, and average pore size, the modified microporous membrane containing hydrophilic ion exchange polymer has better hydrophilicity and shows a smaller contact angle.

[0233] It can be seen from Tables 1 and 2 that compared with e-PTFE-2, the tensile strength of De-PTFE-3 is reduced by more than 50%, the thickness distribution range is wide, and the pore size distribution range is wide. This is because the perfluorosulfonic acid resin solid is unevenly dispersed in PTFE and is difficult to fibrillate.

[0234] Compared with De-PTFE-2, the thickness distribution, pore size distribution and porosity of e-PTFE-2 are similar, and the tensile strength is reduced by about 5%. The introduction of perfluorosulfonic acid resin has a lower effect on the strength of the microporous membrane. This is because the perfluorosulfonic acid resin is evenly dispersed and has a small particle size, and the fibrillation of the composite is less different from that of single polytetrafluoroethylene.

[0235] Figure 2 The surface SEM images of e-PTFE-2, De-PTFE-2 and De-PTFE-3 are shown in Figure 2. The surface SEM images of the two microporous membranes, e-PTFE-2 and De-PTFE-2, are basically the same, and the fiber structure surface is smooth and uniform, indicating that the hydrophilic ion exchange polymer has good dispersion in the skeleton polymer material PTFE and has no adverse effect on subsequent processing and molding. The nodes and fiber structures of De-PTFE-3 are chaotic, which is caused by the poor solid dispersion of the hydrophilic ion exchange polymer.

[0236] Table 3

[0237] Ion exchange membrane Enhancement Layer Average thickness (μm) IEC(mmol / g) PEM-2 e-PTFE-2 12 1.13 PEM-3 e-PTFE-3 5 1.51 PEM-4 e-PTFE-4 25 0.90 PEM-4QA e-PTFE-4QA 25 0.88 PEM-6 e-PTFE-6 100 0.69 D-PEM-2 De-PTFE-2 12 1.11 D-PEM-4 De-PTFE-4 25 1.50

[0238] Table 3 shows the reinforcement layer, average thickness and IEC of the ion exchange membrane. The modified microporous membranes with different material compositions and preparation methods can be composited with ion exchange resins to prepare ion exchange membranes.

[0239] Table 4

[0240]

[0241] Table 4 shows the tensile strength, conductivity and free radical resistance of the ion exchange membrane. The MD and TD directions of the ion exchange membrane are consistent with those of the microporous membrane. Compared with the unmodified microporous membrane, the modified microporous membrane containing the hydrophilic ion exchange polymer has better free radical resistance and lower mass loss in the corresponding stability test when the ion exchange membrane is prepared by the same ion exchange resin and process. The strength of the modified microporous membrane is slightly lower than that of the unmodified microporous membrane, but the electrochemical and mechanical properties of the ion exchange membrane prepared by the modified microporous membrane are better than those of the ion exchange membrane prepared by the unmodified microporous membrane. The introduction of the hydrophilic ion exchange polymer improves the hydrophilicity of the microporous membrane, which is beneficial to the infiltration of the ion exchange resin, so that the ion exchange resin is more fully filled in the microporous membrane, which is beneficial to the improvement of conductivity, tensile strength and barrier properties. The surface of e-PTFE-4QA in PEM-4QA contains alkaline quaternary ammonium groups, which will form ionic crosslinks with the sulfonic acid groups in the ion exchange resin. This ionic crosslinking can further enhance the bonding effect between the resin matrix and the reinforcement layer fibers, thereby improving the barrier properties and dimensional stability of the composite membrane.

[0242] Fiber reinforcement is the key to improving the strength of ion exchange membranes. The tensile strength of PEM-4, PEM-4QA and D-PEM-4 with e-PTFE membrane reinforcement layer is much higher than that of D-PEM-4C, D-PEM-4F and M-PTFE without fiber reinforcement structure. Whether it is a single ion exchange resin membrane, a single polytetrafluoroethylene membrane or a composite membrane of ion exchange resin and polytetrafluoroethylene, the mechanical strength is low without fiber structure, and the application scenarios are limited.

[0243] Figure 3 The cross-sectional SEM images of PEM-2 and D-PEM-2 show that PEM-2 has better filling of ion exchange resin at the reinforcement layer than D-PEM-2.

[0244] Figure 4 Polarization curves of PEM-2 and D-PEM-2. The power density of the membrane electrode prepared by PEM-2 reaches 1425mW / cm 2 @0.65V, better than D-PEM-2’s 1363mW / cm 2 @0.65V, with higher fuel cell single cell performance. The average hydrogen permeation current of PEM-2 is 2.6mA / cm 2 @0.4V, lower than 3.9mA / cm of D-PEM-2 2 @0.4V, showing better barrier properties.

[0245] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0246] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A microporous membrane, characterized in that: The invention comprises polytetrafluoroethylene and a hydrophilic ion exchange polymer, wherein the hydrophilic ion exchange polymer comprises at least one of a hydrophilic anion exchange polymer or a hydrophilic cation exchange polymer.

2. The microporous membrane according to claim 1, characterized in that The hydrophilic anion exchange polymer includes a perfluoroazonium ion resin; and / or, the hydrophilic cation exchange polymer comprises at least one of a sulfonated polymer, a perfluorosulfonyl imide resin or a phosphonated polymer; And / or, the mass ratio of the polytetrafluoroethylene to the hydrophilic ion exchange polymer is 100:0.01-25.

3. The microporous membrane according to claim 1 or 2, characterized in that: The average pore size of the microporous membrane is 0.01 to 1 μm; and / or, the porosity of the microporous membrane is 30 to 95%; And / or, the microporous membrane has a thickness of 1 to 1000 μm.

4. A method for preparing a microporous membrane according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) blending a polytetrafluoroethylene emulsion and a hydrophilic ion exchange polymer to obtain a composite; (2) Forming the composite into a film to obtain a microporous membrane.

5. The method for preparing a microporous membrane according to claim 4, characterized in that: In the step (1), the mass percentage concentration of the polytetrafluoroethylene emulsion is 5% to 90%; And / or, in the step (1), the hydrophilic ion exchange polymer and the polytetrafluoroethylene emulsion are uniformly mixed, and then co-coagulated and / or dried to obtain a composite; And / or, in step (1), the particle size of the composite is ≤4 mm; And / or, in the step (2), the film is formed by biaxial stretching; the biaxial stretching includes MD direction stretching and TD direction stretching, the MD direction stretching multiple is 2 to 15; the TD direction stretching multiple is 2 to 45.

6. An ion exchange membrane, characterized in that: The invention comprises an ion exchange resin and a microporous membrane, wherein the microporous membrane is the microporous membrane described in any one of claims 1 to 3 or the microporous membrane prepared by the preparation method described in claim 4 or 5.

7. The ion exchange membrane according to claim 6, characterized in that The thickness of the ion exchange membrane is 3 μm to 500 μm; And / or, the ion exchange capacity of the ion exchange membrane is 0.1 mmol / g to 5.2 mmol / g.

8. A method for preparing an ion exchange membrane according to claim 6 or 7, characterized in that: The following steps are involved: 1) dispersing an ion exchange resin in a solvent to obtain an ion exchange resin dispersion; 2) coating the ion exchange resin dispersion on one side or both sides of a microporous membrane and drying the membrane to obtain an ion exchange membrane.

9. Use of the microporous membrane according to any one of claims 1 to 3 or the ion exchange membrane according to claim 6 or 7, characterized in that: Used for at least one of filtering, separation, sealing material, and textile material.

10. The use according to claim 9, characterized in that: Used in at least one of fuel cells, water electrolysis, flow batteries, chlor-alkali industry, electrodialysis or osmosis.