Hexavalent chromium-phosphorus synchronous chemical removal nano composite material and preparation method thereof
By preparing hexavalent chromium-phosphorus synchronous chemical removal nanocomposites, the reduction, oxidation and flocculation mechanism of Fe@SiO2-CaO composites is solved, and the problem of difficulty in removing hexavalent chromium and phosphate in composite wastewater in the prior art is solved. , realizes efficient removal of heavy metals, nutrients and organic pollutants, and is suitable for large-scale sewage treatment.
Patent Information
- Application Number
- CN202410958761.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to effectively remove a variety of pollutants such as hexavalent chromium (Cr(VI) and phosphate (PO43-) in composite wastewater. Single or composite nanomaterials usually only show excellent performance for specific categories of pollutants. , It is difficult to completely remove all kinds of pollutants in composite sewage.
The preparation method of synchronous chemical removal of nanocomposites by hexavalent chromium-phosphorus synchronous chemical removal of nanocomposites is adopted. Nanocalcium oxide is produced by reacting calcium chloride with alkali liquid and oxidizing agent, and then ultrasonic treatment is carried out in the ethanol-water mixed solution and ammonia and tetraethylene are added. The oxysilane is then added with sodium borohydride and ferric chloride solution under the protection of inert gas to form a Fe@SiO2-CaO composite material to achieve efficient removal of Cr(VI) and PO43-.
The method is cleverly designed, simple in process, simple in operation, low production cost, can effectively remove Cr(VI) and PO43-, and realizes efficient treatment of composite wastewater containing heavy metals, nutrients and organic pollutants. It is suitable for large-scale promotion. application.
Smart Images

Figure CN118925658A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental protection, more specifically, to the technical field of hexavalent chromium-phosphorus chemical removal in wastewater, and in particular to a hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material and a preparation method thereof. Background Art
[0002] The rapid advancement of industrialization and economic development has led to serious water shortages and water pollution, which seriously restricts the sustainable development of human society. Many pollutants such as pesticides, heavy metals and phosphorus have flowed into water bodies in large quantities, causing serious pollution of water resources and posing huge risks to human health. Effective management of water resources and recycling of sewage have become important means to solve the global water shortage.
[0003] In recent years, people have conducted a lot of research and practice in the fields of coagulation and sedimentation, sand filtration, nitrifying bacteria activated sludge, adsorption, biological treatment, membrane separation, advanced oxidation and other technologies. However, these single technical means are usually difficult to effectively remove various pollutants in complex wastewater, and multiple technologies need to be connected in series to meet the effluent water quality standards. In order to simplify the process, reduce energy consumption, capital cost and floor space, it is urgent to develop new technical solutions that can remove multiple pollutants at the same time.
[0004] Nanomaterials have shown broad application prospects in sewage treatment due to their unique physical and chemical properties, such as small size, large specific surface area and abundant active sites. However, existing single or composite nanomaterials can usually only show excellent performance against specific types of pollutants, and it is difficult to comprehensively remove various pollutants in complex sewage. Therefore, the development of multifunctional nanocomposite materials with reduction, oxidation and flocculation functions is of great significance for expanding the application of nanotechnology in the field of sewage treatment, and also provides innovative technical solutions for solving the global water shortage.
[0005] Therefore, it is desirable to provide a hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material that can effectively remove Cr(VI) and PO4 3- , can be widely used in the treatment of complex wastewater containing heavy metals, nutrients and organic pollutants. Summary of the invention
[0006] In order to overcome the shortcomings of the above-mentioned prior art, an object of the present invention is to provide a hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material, which can effectively remove Cr(VI) and PO4 3- It can be widely used in the treatment of complex wastewater containing heavy metals, nutrients and organic pollutants, and is suitable for large-scale promotion and application.
[0007] Another object of the present invention is to provide a method for preparing a hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material, which has ingenious design, simple process, easy operation, low production cost, and is suitable for large-scale promotion and application.
[0008] To achieve the above object, in a first aspect of the present invention, a method for preparing a hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material is provided, which is characterized in that it comprises the following steps:
[0009] (1) dissolving calcium chloride in water, adding alkali solution and oxidant dropwise while stirring, and continuing stirring to react, centrifuging to obtain a first precipitate after the reaction, washing the first precipitate and freeze-drying it to obtain nano calcium oxide;
[0010] (2) dispersing the nano calcium oxide in an ethanol-water mixed solution, subjecting it to ultrasonic treatment, then dropping ammonia water and tetraethoxysilane to react, centrifuging after the reaction to obtain a second precipitate, washing the second precipitate and freeze-drying it to obtain SiO2-coated nano calcium oxide SiO2-CaO;
[0011] (3) The SiO2-CaO is dispersed in ethanol, subjected to ultrasonic treatment, and then a sodium borohydride ethanol solution is added and stirred for reaction to obtain a NaBH4 ethanol solution of SiO2-CaO. Subsequently, under the protection of an inert gas, a ferric chloride ethanol solution is added dropwise to the pre-deoxygenated NaBH4 ethanol solution of SiO2-CaO, and a third precipitate is obtained by centrifugation. The third precipitate is washed and freeze-dried to obtain a Fe@SiO2-CaO composite material, which is the hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material.
[0012] Preferably, in step (1), the weight of calcium chloride is 10 g, the volume of water is 300 mL, the stirring rate is 700 rpm, the volume of alkali solution is 15 mL, the volume of oxidant is 10 mL, and the continuous stirring time is 3 hours.
[0013] Preferably, in step (1), the alkali solution is selected from at least one of NaOH, KOH and ammonia water.
[0014] Preferably, in step (1), the oxidant is selected from at least one of hydrogen peroxide, potassium permanganate and potassium dichromate.
[0015] Preferably, in step (1), the water is ultrapure water.
[0016] Preferably, in step (2), the weight of the nano-calcium oxide is 5 grams, the volume of the ethanol-water mixed solution is 300 mL, the time of the ultrasonic treatment is 10 minutes, the volume of the ammonia water is 2 mL, the volume of the tetraethoxysilane is 8 mL, and the reaction time is 2 hours.
[0017] Preferably, in step (2), the volume ratio of ethanol to water in the ethanol-water mixed solution is 1 to 5:1.
[0018] Preferably, in the step (3), the weight of the SiO2-CaO is 5 grams, the volume of the ethanol is 200 mL, the time of the ultrasonic treatment is 3 minutes, the concentration of the sodium borohydride ethanol solution is 8 g / L, the volume of the sodium borohydride ethanol solution is 150 mL, the stirring time is 10 minutes, the concentration of the pre-deoxygenated SiO2-CaO NaBH4 ethanol solution is 25 g / L, the volume of the pre-deoxygenated SiO2-CaO NaBH4 ethanol solution is 200 mL, the concentration of the ferric chloride ethanol solution is 1 g / L, and the volume of the ferric chloride ethanol solution is 100 mL.
[0019] Preferably, in step (3), the inert gas is nitrogen.
[0020] In a second aspect of the present invention, a hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material is provided, wherein the nanocomposite material is prepared by the above-mentioned method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material.
[0021] The beneficial effects of the present invention are:
[0022] 1. The preparation method of the hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material of the present invention comprises: (1) dissolving calcium chloride in water, dripping alkali solution and oxidant while stirring, and continuously stirring to react, centrifuging to obtain a precipitate, washing and freeze-drying to obtain nano calcium oxide; (2) dispersing the nano calcium oxide in an ethanol-water mixed solution, ultrasonically treating, then dripping ammonia water and tetraethoxysilane to react, centrifuging to obtain a precipitate, washing and freeze-drying to obtain SiO2-coated nano calcium oxide SiO2-CaO; (3) dispersing SiO2-CaO in ethanol, ultrasonically treating, then adding sodium borohydride ethanol solution, stirring to react, obtaining NaBH4 ethanol solution of SiO2-CaO, then dripping ferric chloride ethanol solution into the pre-deoxidized NaBH4 ethanol solution of SiO2-CaO under the protection of inert gas, centrifuging to obtain a precipitate, washing and freeze-drying. Therefore, the method has ingenious design, simple process, easy operation, low production cost and is suitable for large-scale promotion and application.
[0023] 2. The hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material of the present invention is prepared by the above-mentioned hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material preparation method, so it can effectively remove Cr(VI) and PO4 3- It can be widely used in the treatment of complex wastewater containing heavy metals, nutrients and organic pollutants, and is suitable for large-scale promotion and application.
[0024] These and other objects, features and advantages of the present invention will be more fully reflected in the following detailed description and claims, and may be achieved by the means, devices and combinations thereof particularly pointed out in the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a scanning electron microscope image of the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material prepared in Example 1.
[0026] Figure 2 This is a graph showing the change in P removal rate of the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material for Cr(VI) prepared in Example 1 as a function of the amount of nanocomposite material added.
[0027] Figure 3 This is a graph showing the change in removal rate of Cr(VI) and P over time for the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material prepared in Example 1. DETAILED DESCRIPTION
[0028] In order to provide a hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material, which can effectively remove Cr(VI) and PO4 3- , which can be widely used in the treatment of composite wastewater containing heavy metals, nutrients and organic pollutants. The inventors have obtained a method for preparing a hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material through in-depth and extensive research. The hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material prepared by the method can effectively remove Cr(VI) and PO4 3- , can be widely used in the treatment of complex wastewater containing heavy metals, nutrients and organic pollutants.
[0029] The preparation method of the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material of the present invention comprises the following steps:
[0030] (1) dissolving calcium chloride in water, adding alkali solution and oxidant dropwise while stirring, and continuing stirring to react, centrifuging to obtain a first precipitate after the reaction, washing the first precipitate and freeze-drying it to obtain nano calcium oxide;
[0031] (2) dispersing the nano calcium oxide in an ethanol-water mixed solution, subjecting it to ultrasonic treatment, then dropping ammonia water and tetraethoxysilane to react, centrifuging after the reaction to obtain a second precipitate, washing the second precipitate and freeze-drying it to obtain SiO2-coated nano calcium oxide SiO2-CaO;
[0032] (3) The SiO2-CaO is dispersed in ethanol, subjected to ultrasonic treatment, and then a sodium borohydride ethanol solution is added and stirred for reaction to obtain a NaBH4 ethanol solution of SiO2-CaO. Subsequently, under the protection of an inert gas, a ferric chloride ethanol solution is added dropwise to the pre-deoxygenated NaBH4 ethanol solution of SiO2-CaO, and a third precipitate is obtained by centrifugation. The third precipitate is washed and freeze-dried to obtain a Fe@SiO2-CaO composite material, which is the hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material.
[0033] In the step (1), the weight of the calcium chloride, the volume of the water, the stirring rate, the volume of the alkali solution, the volume of the oxidant and the continuous stirring time can be determined as needed. Preferably, in the step (1), the weight of the calcium chloride is 10 grams, the volume of the water is 300 mL, the stirring rate is 700 rpm, the volume of the alkali solution is 15 mL, the volume of the oxidant is 10 mL, and the continuous stirring time is 3 hours.
[0034] In the step (1), the alkali solution may be any suitable alkali solution. Preferably, in the step (1), the alkali solution is selected from at least one of NaOH, KOH and ammonia water.
[0035] In the step (1), the oxidant may be any suitable oxidant. Preferably, in the step (1), the oxidant is selected from at least one of hydrogen peroxide, potassium permanganate and potassium dichromate.
[0036] In the step (1), the water may be any suitable water. Preferably, in the step (1), the water is ultrapure water.
[0037] In the step (2), the weight of the nano-calcium oxide, the volume of the ethanol-water mixed solution, the time of the ultrasonic treatment, the volume of the ammonia water, the volume of the tetraethoxysilane and the reaction time can be determined as needed. Preferably, in the step (2), the weight of the nano-calcium oxide is 5 grams, the volume of the ethanol-water mixed solution is 300 mL, the time of the ultrasonic treatment is 10 minutes, the volume of the ammonia water is 2 mL, the volume of the tetraethoxysilane is 8 mL, and the reaction time is 2 hours.
[0038] In the step (2), the volume ratio of ethanol to water in the ethanol-water mixed solution can be determined as needed. Preferably, in the step (2), the volume ratio of ethanol to water in the ethanol-water mixed solution is 1 to 5:1.
[0039] In the step (3), the weight of the SiO2-CaO, the volume of the ethanol, the time of the ultrasonic treatment, the concentration of the sodium borohydride ethanol solution, the volume of the sodium borohydride ethanol solution, the stirring time, the concentration of the NaBH4 ethanol solution of the pre-deoxidized SiO2-CaO, the volume of the NaBH4 ethanol solution of the pre-deoxidized SiO2-CaO, the concentration of the ferric chloride ethanol solution and the volume of the ferric chloride ethanol solution can be determined as needed. Preferably, in the step (3), the SiO2-CaO The weight is 5 grams, the volume of ethanol is 200 mL, the time of ultrasonic treatment is 3 minutes, the concentration of the sodium borohydride ethanol solution is 8 g / L, the volume of the sodium borohydride ethanol solution is 150 mL, the stirring time is 10 minutes, the concentration of the NaBH4 ethanol solution of pre-deoxidized SiO2-CaO is 25 g / L, the volume of the NaBH4 ethanol solution of pre-deoxidized SiO2-CaO is 200 mL, the concentration of the ferric chloride ethanol solution is 1 g / L, and the volume of the ferric chloride ethanol solution is 100 mL.
[0040] In the step (3), the inert gas may be any suitable inert gas. Preferably, in the step (3), the inert gas is nitrogen.
[0041] The washing can be performed using any suitable reagent, preferably, the washing is performed using ethanol.
[0042] The present invention also provides a hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material, which is prepared by adopting the above-mentioned method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material.
[0043] In order to more clearly understand the technical content of the present invention, the following embodiments are given in detail.
[0044] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards. If there are no corresponding national standards, they are carried out according to the general international standards, conventional conditions, or conditions recommended by the manufacturer.
[0045] Unless otherwise defined or indicated, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the method of the present invention.
[0046] Example 1
[0047] In this embodiment, hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material I is prepared by the following scheme.
[0048] Step S1: 10 g of calcium chloride was dissolved in 300 mL of ultrapure water, and 15 mL of ammonia and 10 mL of hydrogen peroxide were added dropwise under constant stirring at 700 rpm, and stirring was continued for 3 hours. After centrifugation for 20 minutes, the precipitated particles were washed with ethanol and freeze-dried for 24 hours to obtain nano calcium oxide;
[0049] Step S2: Disperse 5 g of nano-calcium oxide in 300 mL of ethanol-water mixed solution (the volume ratio of ethanol to water is 1:1), and treat with ultrasound for 10 minutes. Then, add 2 mL of ammonia water and 8 mL of tetraethoxysilane (TEOS) dropwise, and react for 2 hours. Centrifuge to obtain a precipitate, wash with ethanol, and freeze-dry for 12 hours to obtain SiO2-coated nano-calcium oxide (SiO2-CaO);
[0050] Step S3: 5g SiO2-CaO was dispersed in 200mL ethanol, ultrasonically treated for 3 minutes, and then 150mL of 8g / L sodium borohydride ethanol solution was added and stirred for 10 minutes. Under nitrogen protection, 100mL of 1g / L ferric chloride ethanol solution was slowly added to 200mL 25g / L NaBH4 ethanol solution of SiO2-CaO that was pre-deoxygenated (inert gas deoxygenation). After centrifugation for 20 minutes and vacuum freeze drying for 24 hours, Fe@SiO2-CaO composite material I, i.e. hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material I, was obtained.
[0051] The scanning electron microscope image of hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material Ⅰ is shown in Figure 1 As shown (using German Zeiss SIGMA300 field emission electron microscope).
[0052] Example 2
[0053] In this embodiment, hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material II is prepared by the following scheme.
[0054] Step S1: 10 g of calcium chloride was dissolved in 300 mL of ultrapure water, and 15 mL of NaOH and 10 mL of hydrogen peroxide were added dropwise under constant stirring at 700 rpm, and stirring was continued for 3 hours. After centrifugation for 20 minutes, the precipitated particles were washed with ethanol and freeze-dried for 24 hours to obtain nano calcium oxide;
[0055] Step S2: Disperse 5 g of nano-calcium oxide in 300 mL of ethanol-water mixed solution (the volume ratio of ethanol to water is 5:1), and treat with ultrasound for 10 minutes. Then, add 2 mL of ammonia water and 8 mL of tetraethoxysilane (TEOS) dropwise, and react for 2 hours. Centrifuge to obtain a precipitate, wash with ethanol, and freeze-dry for 12 hours to obtain SiO2-coated nano-calcium oxide (SiO2-CaO);
[0056] Step S3: 5g SiO2-CaO was dispersed in 200mL ethanol, ultrasonically treated for 3 minutes, and then 150mL of 8g / L sodium borohydride ethanol solution was added and stirred for 10 minutes. Under nitrogen protection, 100mL of 1g / L ferric chloride ethanol solution was slowly added to 200mL 25g / L NaBH4 ethanol solution of SiO2-CaO that was pre-deoxygenated (inert gas deoxygenation). After centrifugation for 20 minutes and vacuum freeze drying for 24 hours, Fe@SiO2-CaO composite material II, i.e. hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material ⅠI, was obtained.
[0057] Example 3
[0058] In this embodiment, hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material III is prepared by the following scheme.
[0059] Step S1: 10 g of calcium chloride was dissolved in 300 mL of ultrapure water, and 15 mL of NaOH and 10 mL of potassium permanganate aqueous solution were added dropwise under constant stirring at 700 rpm, and stirring was continued for 3 hours. After centrifugation for 20 minutes, the precipitated particles were washed with ethanol and freeze-dried for 24 hours to obtain nano calcium oxide;
[0060] Step S2: Disperse 5 g of nano-calcium oxide in 300 mL of ethanol-water mixed solution (volume ratio of ethanol to water is 1.5:1), and treat with ultrasound for 10 minutes. Then, add 2 mL of ammonia water and 8 mL of tetraethoxysilane (TEOS) dropwise, and react for 2 hours. Centrifuge to obtain a precipitate, wash with ethanol, and freeze-dry for 12 hours to obtain SiO2-coated nano-calcium oxide (SiO2-CaO);
[0061] Step S3: 5g SiO2-CaO was dispersed in 200mL ethanol, ultrasonically treated for 3 minutes, and then 150mL of 8g / L sodium borohydride ethanol solution was added and stirred for 10 minutes. Under nitrogen protection, 100mL of 1g / L ferric chloride ethanol solution was slowly added to 200mL 25g / L NaBH4 ethanol solution of SiO2-CaO that was pre-deoxygenated (inert gas deoxygenation). After centrifugation for 20 minutes and vacuum freeze drying for 24 hours, Fe@SiO2-CaO composite material III, i.e. hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material III, was obtained.
[0062] Example 4
[0063] In this embodiment, hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material IV is prepared by the following scheme.
[0064] Step S1: 10 g of calcium chloride was dissolved in 300 mL of ultrapure water, and 15 mL of KOH and 10 mL of potassium dichromate aqueous solution were added dropwise under constant stirring at 700 rpm, and stirring was continued for 3 hours. After centrifugation for 20 minutes, the precipitated particles were washed with ethanol and freeze-dried for 24 hours to obtain nano calcium oxide;
[0065] Step S2: Disperse 5 g of nano-calcium oxide in 300 mL of ethanol-water mixed solution (the volume ratio of ethanol to water is 2:1), and treat with ultrasound for 10 minutes. Then, add 2 mL of ammonia water and 8 mL of tetraethoxysilane (TEOS) dropwise, and react for 2 hours. Centrifuge to obtain a precipitate, wash with ethanol, and freeze-dry for 12 hours to obtain SiO2-coated nano-calcium oxide (SiO2-CaO);
[0066] Step S3: 5g SiO2-CaO was dispersed in 200mL ethanol, ultrasonically treated for 3 minutes, and then 150mL of 8g / L sodium borohydride ethanol solution was added and stirred for 10 minutes. Under nitrogen protection, 100mL of 1g / L ferric chloride ethanol solution was slowly added to 200mL 25g / L NaBH4 ethanol solution of SiO2-CaO that was pre-deoxygenated (inert gas deoxygenation). After centrifugation for 20 minutes and vacuum freeze drying for 24 hours, Fe@SiO2-CaO composite material IV, i.e. hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material IV, was obtained.
[0067] Effect Detection Example
[0068] Static adsorption was used to adsorb Cr(VI) and P in the solution using the hexavalent chromium-phosphorus synchronous chemical removal nanocomposites I to IV prepared in Examples 1 to 4, respectively, to investigate the removal effect of the nanocomposites on Cr(VI) and P in the solution. The adsorbed solution was subjected to diphenylcarbohydrazide spectrophotometry (water quality determination of hexavalent chromium diphenylcarbohydrazide spectrophotometry (GB 7467-87)) to determine the Cr(VI) concentration. The adsorbed solution was subjected to ammonium molybdate spectrophotometry (GB11893-89 water quality determination of total phosphorus ammonium molybdate spectrophotometry) to determine the P concentration.
[0069] Hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material Ⅰ For Cr(VI), the change of P removal rate with the addition amount of nanocomposite material is shown in the figure Figure 2 As shown. Hexavalent chromium-phosphorus simultaneous chemical removal of nanocomposites ⅠI~IV For Cr(VI), the change of P removal rate with the addition amount of nanocomposites is similar Figure 2 shown.
[0070] Hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material Ⅰ For Cr(VI), the change of P removal rate over time is shown in the figure Figure 3 As shown. The graph of the change of P removal rate over time for hexavalent chromium-phosphorus simultaneous chemical removal nanocomposites ⅠI~IV is similar to that for Cr(VI). Figure 3 shown.
[0071] Therefore, the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material of the present invention has a core of calcium oxide, a middle layer of silicon dioxide, and an outer layer of zero-valent iron. 0 It has reducing properties and can reduce hexavalent chromium (Cr(VI)) to trivalent chromium (Cr(III)). 0 The hydrogen radical H generated by the reaction with water can also participate in the reduction reaction. The generated Cr(III) reacts with SiO2 and OH - The coprecipitation is formed to remove Cr(VI). The removal of phosphate mainly depends on the coordination precipitation reaction formed with free calcium ions and iron compounds. The slow-release oxidation of the CaO core can also effectively remove organic pollutants in water. The test results show that the hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material of the present invention has a good effect on 30mg / L Cr(VI) and 60mg / L PO4 3- With a removal rate of over 99%, this multifunctional property makes it widely used in the treatment of complex wastewater containing heavy metals, nutrients and organic pollutants.
[0072] Compared with the prior art, the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material of the present invention has the following advantages:
[0073] Strong versatility: Through multiple mechanisms such as reduction, oxidation and flocculation, it can simultaneously remove various pollutants such as heavy metals, nutrients and organic pollutants in the water, achieving comprehensive treatment of complex sewage.
[0074] High removal efficiency: for 30 mg / L hexavalent chromium and 60 mg / L phosphate, the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material of the present invention can achieve a removal rate of more than 99%, showing excellent pollutant removal performance.
[0075] The reaction mechanism is clear: Fe 0 The mechanisms of the reduction of , the participation of ·H radicals in the reaction, the slow-release oxidation of CaO and co-precipitation have been elucidated, providing a theoretical basis for the rational design of materials and performance optimization.
[0076] Broad application prospects: This material can be widely used in the treatment of complex sewage containing heavy metals, nutrients and organic matter, providing an innovative technical solution to the current water pollution problem.
[0077] In summary, the preparation method of the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material of the present invention is ingeniously designed, simple in process, easy to operate, and has low production cost. The prepared hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material can effectively remove Cr(VI) and PO4 3- It can be widely used in the treatment of complex wastewater containing heavy metals, nutrients and organic pollutants, and is suitable for large-scale promotion and application.
[0078] In this specification, the present invention has been described with reference to specific embodiments thereof. However, it is apparent that various modifications and variations may be made without departing from the spirit and scope of the present invention. Therefore, the description should be regarded as illustrative rather than restrictive.
Claims
1. A method for preparing a hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material, characterized in that: The following steps are involved: (1) dissolving calcium chloride in water, adding alkali solution and oxidant dropwise while stirring, and continuing stirring to react, centrifuging to obtain a first precipitate after the reaction, washing the first precipitate and freeze-drying it to obtain nano calcium oxide; (2) dispersing the nano calcium oxide in an ethanol-water mixed solution, subjecting it to ultrasonic treatment, then dropping ammonia water and tetraethoxysilane to react, centrifuging after the reaction to obtain a second precipitate, washing the second precipitate and freeze-drying it to obtain SiO2-coated nano calcium oxide SiO2-CaO; (3) The SiO2-CaO is dispersed in ethanol, subjected to ultrasonic treatment, and then a sodium borohydride ethanol solution is added and stirred for reaction to obtain a NaBH4 ethanol solution of SiO2-CaO. Subsequently, under the protection of an inert gas, a ferric chloride ethanol solution is added dropwise to the pre-deoxygenated NaBH4 ethanol solution of SiO2-CaO, and a third precipitate is obtained by centrifugation. The third precipitate is washed and freeze-dried to obtain a Fe@SiO2-CaO composite material, which is the hexavalent chromium-phosphorus synchronous chemical removal nanocomposite material.
2. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (1), the weight of the calcium chloride is 10 g, the volume of the water is 300 mL, the stirring rate is 700 rpm, the volume of the alkali solution is 15 mL, the volume of the oxidant is 10 mL, and the continuous stirring time is 3 hours.
3. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (1), the alkali solution is selected from at least one of NaOH, KOH and ammonia water.
4. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (1), the oxidant is selected from at least one of hydrogen peroxide, potassium permanganate and potassium dichromate.
5. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (1), the water is ultrapure water.
6. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (2), the weight of the nano-calcium oxide is 5 grams, the volume of the ethanol-water mixed solution is 300 mL, the ultrasonic treatment time is 10 minutes, the volume of the ammonia water is 2 mL, the volume of the tetraethoxysilane is 8 mL, and the reaction time is 2 hours.
7. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (2), the volume ratio of ethanol to water in the ethanol-water mixed solution is 1 to 5:
1.
8. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (3), the weight of the SiO2-CaO is 5 grams, the volume of the ethanol is 200 mL, the time of the ultrasonic treatment is 3 minutes, the concentration of the sodium borohydride ethanol solution is 8 g / L, the volume of the sodium borohydride ethanol solution is 150 mL, the stirring time is 10 minutes, the concentration of the NaBH4 ethanol solution of the pre-deoxygenated SiO2-CaO is 25 g / L, the volume of the NaBH4 ethanol solution of the pre-deoxygenated SiO2-CaO is 200 mL, the concentration of the ferric chloride ethanol solution is 1 g / L, and the volume of the ferric chloride ethanol solution is 100 mL.
9. The method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material according to claim 1, characterized in that: In the step (3), the inert gas is nitrogen.
10. A hexavalent chromium-phosphorus simultaneous chemical removal nanocomposite material, characterized in that: The nanocomposite material is prepared by the method for preparing the hexavalent chromium-phosphorus simultaneous chemical removal according to any one of claims 1 to 9.