Preparation method and application of biochar adsorbent derived from cow dung

The alkali-modified biochar adsorbent is prepared by hydrothermal carbonization and alkali modification treatment of cow dung, which solves the problem of insufficient adsorption performance of cow dung hydrothermal biochar, and achieves efficient removal of cadmium ions in contaminated wastewater, achieving waste resource utilization Targets of utilization and low energy consumption.

CN118925669APending Publication Date: 2024-11-12INNER MONGOLIA UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411216153.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The surface adsorption sites of cow dung hydrothermal biochar are limited, resulting in insufficient adsorption performance and stability, making it difficult to effectively treat industrial wastewater containing cadmium ions.

Method used

Alkaline-modified biochar adsorbent is prepared by hydrothermal carbonization and alkali modification treatment of cow dung. The cadmium ion adsorption performance is improved through pretreatment, hydrothermal carbonization, alkali modification and rinsing steps.

Benefits of technology

The cadmium ion adsorption capacity and stability of biochar adsorbents are significantly improved, and the in-depth treatment of polluted wastewater is achieved, the effect of waste resource utilization is achieved, and the energy consumption for preparation and the generation of polluted gases are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925669A_ABST
    Figure CN118925669A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a biochar adsorbent derived from cow dung, and belongs to the technical field of environmental protection governance, the preparation method comprises the following steps: S1, pretreating dry cow dung to obtain a cow dung precursor; s2, putting the cow dung precursor into a hydrothermal reaction kettle, adding distilled water, performing hydrothermal carbonization treatment, and drying to obtain a carbonized product; s3, dispersing the carbonized product and an alkali modifier in deionized water, and stirring in a water bath for alkali modification treatment to obtain modified charcoal; s4, repeatedly washing the modified biochar with distilled water until the washing liquid is completely neutral, and drying to obtain the biochar adsorbent derived from cow dung. According to the biochar adsorbent for treating the polluted wastewater, the biochar adsorbent for treating the polluted wastewater is fully mixed with the polluted wastewater, and an adsorption reaction is carried out, so that pollutants in the wastewater are adsorbed and removed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental protection and management, and particularly relates to a method for preparing a biochar adsorbent derived from cow dung and application of the biochar adsorbent in adsorbing cadmium ions. Background Art

[0002] With the development of animal husbandry, a large amount of livestock and poultry manure is produced, of which nearly 40% is cow manure. If these livestock and poultry manure are not properly disposed of and randomly piled up, they will inevitably lead to serious environmental and health problems. Therefore, it is particularly important to develop new methods for the disposal of livestock and poultry manure and propose new ways to utilize livestock and poultry manure resources.

[0003] Cadmium is a byproduct of zinc smelting and is widely used in electroplating, chemical, electronics and nuclear industries. Cadmium is also used in batteries, dyes or plastic stabilizer products. During the use of cadmium, a considerable amount of cadmium is discharged into the environment through waste gas, wastewater and waste residue, causing pollution. Cadmium is more easily adsorbed by crops than other heavy metals. The main methods for treating industrial wastewater containing cadmium ions are chemical precipitation, electrolysis, ion exchange and reverse osmosis technology. Among them, the adsorption method has the advantages of high treatment capacity, simple operation and recyclable adsorbent. Especially when treating low-concentration cadmium ion wastewater, its treatment efficiency and operating cost have obvious advantages.

[0004] In recent years, hydrothermal carbonization of cow dung has been studied at home and abroad, making it possible to recycle and utilize cow dung as a resource. However, the surface adsorption sites of cow dung hydrothermal biochar itself are limited, so its adsorption performance and stability are greatly limited. Therefore, it is of great significance to develop a method for preparing cow dung biochar with high adsorption performance and stable properties. Summary of the invention

[0005] In order to solve the problems in the above technical background, the purpose of the present invention is to provide a method for preparing a cow dung-derived biochar adsorbent, wherein the adsorbent is an alkali-modified cow dung biochar to improve its cadmium ion adsorption performance; the method can realize the resource utilization of biomass waste and at the same time deeply treat cadmium-containing wastewater.

[0006] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme: A method for preparing a biochar adsorbent derived from cow dung, such as Figure 1 As shown, the following steps are included: S1. Cow dung pretreatment: pretreating dry cow dung to obtain a cow dung precursor; S2, hydrothermal carbonization: placing the cow dung precursor in a hydrothermal reactor, adding distilled water at a material-liquid mass ratio of 1:8-12, performing hydrothermal carbonization treatment, and performing drying treatment after carbonization to obtain a carbonized product; S3, alkali modification: the prepared carbonization product and the alkali modifier are uniformly dispersed in deionized water, and then ultrasonically treated at 35-45kHZ for 25-35min, and then modified at a water bath temperature of 20-30°C for 10-14h; and stirred in a water bath for alkali modification treatment to obtain modified biochar; S4, rinsing: After the alkali modification treatment is completed, the alkali-modified biochar is repeatedly rinsed with distilled water until the washing liquid becomes completely neutral, and dried at 105° C. for 12 h to obtain the cow dung-derived biochar adsorbent.

[0007] Furthermore, in step S1, the moisture content of the dry cow dung is less than 10%.

[0008] Furthermore, in step S1, the pretreatment method is to grind the dry cow dung to make it pass through a 60-mesh sieve.

[0009] Furthermore, in step S2, the temperature of the hydrothermal carbonization treatment is 200-260°C, the heating rate is 2°C / min, and the carbonization time is 5-7 h.

[0010] Furthermore, in step S2, the temperature of the hydrothermal carbonization treatment is 230°C, the heating rate is 2°C / min, and the carbonization time is 6 h.

[0011] Furthermore, in step S2, the drying process is carried out at a temperature of 105°C and for a time of 12 hours.

[0012] Furthermore, in step S3, the alkaline modifier is any one of potassium hydroxide, sodium hydroxide, sodium carbonate, and sodium bicarbonate.

[0013] Furthermore, in step S3, the temperature of the water bath is 25° C. and the time is 12 h; the amount of the alkali modifier added is such that the mass ratio of carbonized product: alkali modifier is 1:1-1:10.

[0014] Furthermore, the alkali modifier is sodium carbonate, and in step S3, the amount of the alkali modifier added is such that the mass ratio of carbonization product: alkali modifier is 1:4.

[0015] On the other hand, the present invention provides a cow dung-derived biochar adsorbent prepared by a cow dung-derived biochar adsorbent preparation method.

[0016] On the other hand, the present invention provides an application of the cow dung-derived biochar adsorbent, characterized in that it is used to purify cadmium-contaminated wastewater.

[0017] Furthermore, the cadmium-contaminated wastewater is a cadmium ion (Cd 2+ ) wastewater.

[0018] The beneficial effects of the present invention are: 1. The present invention also provides an application of the prepared biochar adsorbent, which is to treat polluted wastewater by adsorption, specifically: providing a biochar adsorbent for treating polluted wastewater; fully mixing the biochar adsorbent for treating polluted wastewater with the polluted wastewater, and performing an adsorption reaction to complete the adsorption and removal of pollutants in the wastewater.

[0019] 2. The present invention uses cow dung to prepare biochar by hydrothermal carbonization and alkali modification, turning waste into treasure and realizing waste resource utilization. In addition, the adsorbent of the present invention prepared with cow dung as raw material is used to remove heavy metals in the solution, achieving the effect of treating waste with waste.

[0020] 3. The present invention adopts a hydrothermal carbonization method to prepare biochar. Compared with the traditional dry distillation preparation method, it has lower energy consumption, simpler processing method, and almost no pollution gas. At the same time, it can better adapt to the resource utilization scenario of waste with high water content. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0022] Figure 1 A process flow chart of a method for preparing a biochar adsorbent derived from cow dung; Figure 2 This is a performance comparison chart of the adsorbents in Examples 1-4 and Comparative Example 1 for the adsorption capacity of cadmium ions; Figure 3 This is a comparison chart of the adsorption capacity of cadmium ions by the adsorbents in Examples 3, 5-7 and Comparative Example 1; Figure 4 FT-IR comparison diagram of Example 5 and Comparative Example 1; Figure 5 This is a SEM comparison diagram of Example 5 and Comparative Example 1. DETAILED DESCRIPTION

[0023] Example 1 Step 1: Weigh an appropriate amount of dry cow dung and grind it through a 60-mesh sieve; Step 2: Place the cow dung treated in step 1 and distilled water in the inner tank of a hydrothermal reactor at a mass ratio of 1:10; then perform hydrothermal carbonization treatment at a hydrothermal temperature of 230 °C, a heating rate of 2 °C / min, and a time of 6 h; after the reaction is completed, dry the carbonized product at 105 °C for 12 h; Step 3: The carbonized product described in step 2 was uniformly mixed with sodium hydroxide in a mass ratio of 1:1, and then treated with ultrasound at 40 kHz for 30 minutes, and then modified in a water bath at 25°C for 12 hours; Step 4: The biochar modified in step 3 is repeatedly rinsed with distilled water until the washing liquid becomes neutral, and then dried at 105 °C for 12 h to obtain a sodium carbonate-modified biochar adsorbent.

[0024] Example 2 The difference from Example 1 is that the alkaline modifier in step 3 is replaced with potassium hydroxide, and the remaining steps and conditions are the same as those in Example 1; that is, a biochar adsorbent modified with potassium hydroxide is obtained.

[0025] Example 3 The difference from Example 1 is that the alkaline modifier in step 3 is replaced with sodium carbonate, and the remaining steps and conditions are the same as those in Example 1; that is, a sodium carbonate-modified biochar adsorbent is obtained.

[0026] Example 4 The difference from Example 1 is that the alkaline modifier in step 3 is replaced with sodium bicarbonate, and the remaining steps and conditions are the same as those in Example 1; that is, a sodium bicarbonate-modified biochar adsorbent is obtained.

[0027] Example 5 The difference from Example 3 is that the mass ratio of the carbonization product to sodium carbonate in Step 3 is increased to 1:4, and the remaining steps and conditions are the same as those in Example 3.

[0028] Example 6 The difference from Example 3 is that the mass ratio of the carbonization product to sodium carbonate in step 3 is increased to 1:2, and the remaining steps and conditions are the same as those in Example 3.

[0029] Example 7 The difference from Example 3 is that the mass ratio of the carbonized product to sodium carbonate in step 3 is increased to 1:10, and the remaining steps and conditions are the same as those in Example 3.

[0030] Comparative Example 1 Weigh an appropriate amount of dry cow dung and grind it through a 60-mesh sieve; The cow dung treated in step 1 and distilled water are placed in the inner tank of a hydrothermal reactor with a mass ratio of 1:10; then a hydrothermal carbonization treatment is carried out with a hydrothermal temperature of 230 °C, a heating rate of 2 °C, and a time of 6 h; after the reaction is completed, the carbonization product is dried at 105 °C for 12 h; thus, an unmodified biochar adsorbent is obtained.

[0031] Comparative Example 2 Different from Example 6, the mass ratio of the carbonized product to sodium carbonate in this comparative example is 1:12.

[0032] Comparative Example 3 Different from Example 7, in step 3: the carbonized product described in step 2 is uniformly mixed with sodium carbonate in a mass ratio of 1:10, without ultrasonic treatment, and then modified in a water bath temperature of 25°C for 12 h.

[0033] Experimental Section 1. Adsorption performance test: 1 g of the biochar adsorbent prepared in Examples 1-7 and Comparative Example 1 was placed in 1 L of cadmium ion wastewater for 24 h to test the adsorption capacity. The adsorption test conditions were 25±1°C and 140 rpm horizontal shaking. 2+ ) The wastewater concentration is 0.2 g / L.

[0034] like Figure 2 As shown, different alkali modifiers can change the adsorption capacity of biochar adsorbent for cadmium ions, and the cadmium ion adsorption capacity of each adsorbent is Example 3> Example 4> Example 2> Example 1> Comparative Example 1. It can be seen from the figure that under the condition of a carbon-base ratio of 1:1, sodium carbonate can significantly improve the cadmium ion adsorption capacity of the biochar adsorbent.

[0035] like Figure 3 As shown in the figure, under the condition of selecting sodium carbonate as the base modification, different carbon-base ratios can improve the adsorption capacity of biochar adsorbent for cadmium ions, and the cadmium ion adsorption capacity of the adsorbents is as follows: Example 5> Example 6> Example 3> Example 7> Comparative Example 3> Comparative Example 2> Comparative Example 1. It can be seen from the figure that when sodium carbonate is used as the base modifier, the carbon-base ratio is 1:4, which is the optimal carbon-base ratio; moreover, ultrasonic treatment can effectively improve the adsorption capacity; no base modification and increasing the amount of base modifier added will affect the adsorption capacity of the adsorbent.

[0036] 2. Characterization: Taking the characterization of Example 5 and Comparative Example 1 as an example, the prepared biochar adsorbent has a porous structure distributed inside and on the surface, wherein the specific surface area is 11.80 m 2 / g, and the pore volume is 0.071 cm 3 / g, and the average pore size is 24.06 nm.

[0037] like Figure 4 As shown, the types of functional groups on the surface of the alkali-modified biochar adsorbent did not change, but its absorption peak intensity increased significantly, and it had a larger number of surface functional groups, which was beneficial to its adsorption of heavy metals.

[0038] like Figure 5As shown in the figure, the unmodified biochar adsorbent has an irregular block-like carbon-based structure with a relatively smooth surface and fewer pores. After alkali modification, the surface morphology of the biochar adsorbent changes from a smooth block-like structure to a rough, regular spherical structure with uniform distribution. In addition, a large number of pores can be observed on its surface.

[0039] In summary, it can be seen from the specific implementation results that the cow dung-derived biochar adsorbent prepared by the present invention has the ability to quickly adsorb and remove cadmium ions in sewage.

[0040] The cow dung-derived biochar adsorbent provided by the present invention has a rapid removal effect on cadmium ions in sewage, has a large specific surface area, a high removal rate, and a simple preparation process, low cost, and is green and efficient, and has potential application value in the treatment of polluted wastewater.

[0041] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a biochar adsorbent derived from cow dung, characterized in that: The steps include: S1. Cow dung pretreatment: pretreating dry cow dung to obtain a cow dung precursor; S2, hydrothermal carbonization: placing the cow dung precursor in a hydrothermal reactor, adding distilled water at a material-liquid mass ratio of 1:8-12, performing hydrothermal carbonization treatment, and performing drying treatment after carbonization to obtain a carbonized product; S3, alkali modification: the prepared carbonization product and the alkali modifier are uniformly dispersed in deionized water, and then ultrasonically treated at 35-45kHZ for 25-35min, and then modified at a water bath temperature of 20-30°C for 10-14h; and stirred in a water bath for alkali modification treatment to obtain modified biochar; S4, rinsing: After the alkali modification treatment is completed, the alkali-modified biochar is repeatedly rinsed with distilled water until the washing liquid is completely neutral, and dried at 105° C. for 12 h to obtain the cow dung-derived biochar adsorbent.

2. The method for preparing a biochar adsorbent derived from cow dung according to claim 1, characterized in that: In step S1, the moisture content of the dry cow dung is less than 10%; the pretreatment method is to grind the dry cow dung to pass through a 60-mesh sieve.

3. The method for preparing a biochar adsorbent derived from cow dung according to claim 1, characterized in that: In step S2, the temperature of the hydrothermal carbonization treatment is 200-260°C, the heating rate is 2°C / min, and the carbonization time is 5-7 h.

4. The method for preparing a biochar adsorbent derived from cow dung according to claim 3, characterized in that: In step S2, the temperature of the hydrothermal carbonization treatment is 230°C, the heating rate is 2°C / min, the carbonization time is 6 h, and the temperature of the drying treatment is 105°C, the time is 12 h.

5. The method for preparing a biochar adsorbent derived from cow dung according to claim 1, characterized in that: In the step S3, the alkaline modifier is any one of potassium hydroxide, sodium hydroxide, sodium carbonate and sodium bicarbonate.

6. The method for preparing a biochar adsorbent derived from cow dung according to claim 1, characterized in that: In the step S3, the temperature of the water bath is 25° C. and the time is 12 h; the amount of the alkali modifier added is such that the mass ratio of carbonized product: alkali modifier is 1:1-1:

10.

7. The method for preparing a biochar adsorbent derived from cow dung according to claim 1, characterized in that: The alkali modifier is sodium carbonate. In step S3, the amount of alkali modifier added is such that the mass ratio of carbonization product: alkali modifier is 1:

4.

8. The cow dung derived biochar adsorbent prepared by the method for preparing a cow dung derived biochar adsorbent according to claims 1-7.

9. The use of the biochar adsorbent derived from cow dung as claimed in claim 8, characterized in that: Used to purify cadmium-contaminated wastewater.

10. The use of the biochar adsorbent derived from cow dung as claimed in claim 9, wherein the cadmium-contaminated wastewater is cadmium ion wastewater with a concentration of 0.2 g / L.

Citation Information

Cited By

  • Preparation method of cow dung biochar briquette fuel

    CN121319990A