Iron-loaded biochar adsorbent as well as preparation method and application thereof

By converting biomass into graphitized carbon materials and embedded in iron ions and coconut shell powder, the porosity and adsorption efficiency of activated carbon are improved, and the problem of insufficient adsorption capacity of activated carbon in the treatment of inorganic phosphorus-containing wastewater is solved, and efficient wastewater is achieved Treatment and recycling of adsorbents.

CN118925670APending Publication Date: 2024-11-12HEBEI AGRICULTURAL UNIV.
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411219023.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The adsorption capacity of existing activated carbons is weak in the purification treatment of inorganic phosphorus-containing wastewater, and the adsorption capacity and efficiency of existing phosphorus-removing activated carbons still need to be improved.

Method used

By converting biomass into graphitized carbon materials and embed iron ions and coconut shell powder into graphite block materials through electrification and pressurization, the porosity and adsorption capacity of biochar are enhanced and the magnetic separation effect is increased.

Benefits of technology

The phosphorus and heavy metal adsorption efficiency in wastewater was significantly improved, and the PO43-removal rate of more than 98% and the adsorption capacity of more than 49 mg/g was achieved. The absorption of adsorbents was recovered through the introduction of magnetic substances, saving costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of sewage treatment, and particularly discloses an iron-loaded biochar adsorbent as well as a preparation method and application thereof. The preparation method comprises the following steps: adding biomass into an acid solution for dipping to obtain a carbon source; the carbon source is rapidly heated for first roasting, and a graphitized carbon material is obtained; mixing the graphitized carbon material, polyvinyl alcohol and water, and pressing to obtain a graphite blocky material; taking the graphite blocky material as one end of an electrode, putting the graphite blocky material and a platinum electrode into a soluble ferric salt solution, adding coconut shell powder, electrifying and pressurizing to obtain a biochar precursor material; and performing secondary roasting on the biochar precursor material, and crushing to obtain the iron-loaded biochar adsorbent. The biomass is converted into the graphitized carbon material through a specific treatment mode, and the iron ions and the coconut shell powder are embedded into the graphite blocky material by adopting an electrifying and pressurizing mode, so that the porosity of the biochar is improved, and the adsorption capacity and the adsorption efficiency of the biochar are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sewage treatment, and in particular to an iron-loaded biochar adsorbent and a preparation method and application thereof. Background Art

[0002] At present, wastewater phosphorus removal technologies at home and abroad are mainly divided into two categories: biological phosphorus removal and physicochemical phosphorus removal. Physicochemical phosphorus removal can be further divided into chemical precipitation, electrocoagulation, crystallization, adsorption, etc. Among them, adsorption phosphorus removal technology has been widely used in phosphorus removal due to its large capacity, rich adsorbent active points, low energy consumption, low pollution, high efficiency and speed, easy operation, recyclable and low cost. Adsorption phosphorus removal technology uses certain porous or large specific surface area materials to achieve the phosphorus removal process of wastewater mainly through the surface precipitation, ion exchange or attachment adsorption of phosphorus on the surface of the adsorbent; using the adsorption-desorption method, it can simultaneously achieve the elimination of phosphorus pollution and the recovery of phosphorus resources.

[0003] As an adsorbent, activated carbon has a large specific surface area and pore volume, and is widely used in the treatment of organic wastewater and heavy metal wastewater. However, activated carbon has a weak adsorption capacity for inorganic pollutants, which limits its application in the purification of inorganic phosphorus-containing wastewater. The existing technology changes the physicochemical properties of the activated carbon surface by loading a layer of highly active substances different from the activated carbon body (the loaded active substances are mostly metal oxides) on the surface of the activated carbon, increasing its surface active sites, thereby improving the adsorption capacity of the activated carbon. However, the adsorption capacity and efficiency of existing phosphorus removal activated carbon still need to be improved. Summary of the invention

[0004] In view of the above problems, the present invention provides an iron-loaded biochar adsorbent and a preparation method and application thereof. The present invention converts biomass into graphitized carbon material through a specific treatment method, and embeds iron ions and coconut shell powder into the graphite block material by applying electricity and pressure, thereby further improving the porosity of the biochar, increasing the adsorption capacity and adsorption efficiency of the biochar, and achieving the magnetic separability effect of the adsorbent.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a method for preparing an iron-loaded biochar adsorbent, comprising the following steps: S1, adding biomass into an acid solution for impregnation to obtain a carbon source; S2, heating the carbon source to 1000° C. to 1100° C. at a rate of 30° C. / min to 40° C. / min for a first calcination to obtain a graphitized carbon material; S3, mixing the graphitized carbon material, polyvinyl alcohol and water, and pressing to obtain a graphite block material; S4, placing the graphite block material as one end of an electrode together with a platinum electrode into a soluble iron salt solution, adding coconut shell powder, and applying electricity and pressure to obtain a biochar precursor material; The soluble iron salt solution includes divalent iron salt and trivalent iron salt; S5, performing a second calcination on the biochar precursor material, and crushing the biochar precursor material to obtain an iron-loaded biochar adsorbent.

[0006] Compared with the prior art, the preparation method of the iron-loaded biochar adsorbent provided by the present invention first performs acid leaching on the biomass to remove impurities (including ash and organic matter) on the surface or inside of the biomass and purify the biomass; then the obtained carbon source is rapidly heated and first roasted at a specific temperature. The rapid heating method is conducive to the rapid evaporation of chemical moisture and mechanical moisture on the surface or inside of the carbon source, so as to avoid the adverse effect of the first roasting effect caused by the steam pressure generated by these moisture at high temperature; the carbon source is first roasted under specific conditions to form a graphitized carbon material with a large and uniform pore volume, and more oxygen-containing functional groups are introduced, which provides space for the combination of iron ions and internal oxygen-containing groups in the subsequent process; then the graphitized carbon material is pressed into shape, and polyvinyl alcohol is used as a binder, which can ensure that the graphitized carbon material, coconut shell powder and iron ions have a certain bonding effect in the subsequent power-on pressurization, second roasting and crushing process, thereby increasing the bonding force between the materials; there are graphitized carbon materials that can be ionized In order to overcome the interaction force between the iron ions and the coconut shell powder and the graphite block material, the present invention applies a certain voltage to the graphite block material in the soluble iron salt solution, and the potential on the positive electrode will attract the cations of the negative electrode to move toward the positive electrode. Near the negative electrode, the cations will exchange with the cations in the interlayer domain, so that the iron ions and the coconut shell powder are embedded in the interlayer structure of the graphite block material and enter the inner pores of the graphitized carbon material. By utilizing the interaction between the positively charged iron ions and the negatively charged oxygen-containing ions, the iron ions are introduced at specific sites inside the graphite block material, so that the entire layered structure expands or expands, thereby improving the porosity of the biochar, which is more conducive to the subsequent iron-loaded biochar adsorbent to adsorb phosphorus or heavy metal substances in the sewage; the biochar precursor material is subjected to a second roasting to convert the iron ions into iron oxide compounds (including iron oxide and ferroferric oxide) with certain magnetic properties and phosphorus removal effects. At the same time, the coconut shell powder will be partially carbonized, which increases the porosity of the adsorbent and assists in exerting a certain adsorption effect.

[0007] The soluble iron salt solution of the present invention contains both divalent iron salt and trivalent iron salt. The trivalent iron ions are flocculated under acidic conditions (the soluble iron salt solution is acidic), which can be used to regulate the iron ions (including Fe 2+ and Fe 3+) The rate and proportion of embedding into the graphite block material. Coconut shell has a specific structure, which is mainly composed of an outer cellulose layer, a middle hard shell layer and an inner soft shell layer. Among them, the cellulose layer is composed of fibrous cells and has good flexibility, the hard shell layer has high hardness and impact resistance, and the soft shell layer has a certain buffering effect. The present invention introduces coconut shell powder during the power-on and pressurization process. The coconut shell powder of the hard shell layer can serve as a supporting skeleton of the graphite block material. Under the action of voltage, it can be inserted into the interlayer of the graphite block material together with iron ions to form an intercalation composite, which plays a "pillar" effect, prevents collapse between graphitized carbon materials, reinforces the interlayer, and strengthens the effect; the coconut shell powder of the cellulose layer and the soft shell layer is rich in cellulose, and there is a strong interaction force between the molecular chains, which can further improve the stability of the iron-loaded biochar adsorbent.

[0008] In addition, the iron-carrying biochar adsorbent prepared by the present invention is coated with magnetic material ferroferric oxide, and the iron-carrying biochar adsorbent can be recycled in sewage treatment through magnetic attraction, saving costs. The biomass and coconut shell powder in the present invention are solid wastes. The present invention adopts a specific preparation method to reasonably and effectively utilize the above solid wastes to avoid environmental pollution.

[0009] Preferably, in S1, the biomass is selected from plant straw, branches, waste wood or flowers and plants.

[0010] For example, in S1, the biomass needs to be crushed before being added to the acid solution, and the particle size of the biomass after crushing is ≤1 cm.

[0011] Preferably, in S1, the pH of the acid solution is 2-4.

[0012] For example, in S1, the acid solution is selected from hydrochloric acid solution, nitric acid solution or sulfuric acid solution.

[0013] Preferably, in S1, the mass volume ratio of the biomass to the acid solution is 1 g: (6-10) mL.

[0014] Preferably, in S1, the immersion temperature is 5°C to 40°C, and the immersion time is 7h to 8h.

[0015] For example, in S1, after the soaking is completed, the soaked biomass is washed with hot water (70°C-80°C) to obtain a carbon source.

[0016] By limiting the conditions of S1, the present invention can further remove impurities such as ash and organic matter on the surface and inside of the biomass, thereby further improving the purity of the biomass.

[0017] Preferably, in S2, the first calcination time is 2h~3h.

[0018] For example, in S2, after the first calcination is completed, the carbon source after the first calcination is crushed to obtain a graphitized carbon material.

[0019] Preferably, in S3, the mass ratio of the graphitized carbon material, the polyvinyl alcohol and the water is 100:(3-5):(1-1.5).

[0020] Preferably, in S3, the pressing temperature is 60° C. to 80° C., the pressing pressure is 25 MPa to 30 MPa, and the holding time is 3 s to 4 s.

[0021] The present invention limits the amount of polyvinyl alcohol and the pressing conditions, so that the bonding effect of polyvinyl alcohol can be better exerted, so that the graphitized carbon material, coconut shell powder and iron ions have a certain bonding effect, and the adsorption effect of the nano material is not affected; in addition, the preferred pressing conditions can also better press the graphitized carbon material into a shape, thereby forming a graphite block material that is conducive to subsequent power-on and pressurization, and while ensuring the forming rate, it is conducive to the subsequent iron ions and coconut shell powder entering the graphite block material under specific power-on and pressurization conditions.

[0022] For example, in S3, the shape of the graphite block material can be a circular ring or a cylindrical structure. For example, the outer diameter of the circular ring is 200 mm and the inner diameter is 150 mm; the diameter of the cylindrical shape is 50 mm to 100 mm and the length is 150 mm to 200 mm; the length and width of the rectangular parallelepiped are both 50 mm to 100 mm and the length is 150 mm to 200 mm.

[0023] Preferably, in S4, the concentration of the divalent iron salt in the soluble iron salt solution is 0.2 mol / L to 0.3 mol / L, and the concentration of the trivalent iron salt is 0.3 mol / L to 0.4 mol / L.

[0024] Preferably, in S4, the pH value of the soluble iron salt solution is 5-5.5. The pH value of the soluble iron salt solution is adjusted using hydrochloric acid, sulfuric acid or sodium hydroxide.

[0025] Preferably, in S4, the divalent iron salt is ferrous sulfate, and the trivalent iron salt is ferric chloride.

[0026] The present invention can ensure the rate and proportion of iron ions embedded in the graphite block material by limiting the concentration of divalent iron salt and trivalent iron salt and the pH value of the soluble iron salt solution, thereby controlling the pore volume and porosity of the finished iron-carrying biochar adsorbent and increasing the adsorption effect on sewage treatment. The present invention does not limit the amount of the soluble iron salt solution, and it can immerse the graphite block material and the platinum electrode.

[0027] Preferably, in S4, the particle size of the coconut shell powder is 5 μm to 10 μm.

[0028] Preferably, in S4, the mass ratio of the graphite block material to the coconut shell powder is 100:(10-20).

[0029] The present invention can further exert the supporting and stabilizing effects of coconut shell powder by limiting the particle size and dosage of coconut shell powder, and coconut shell powder with a specific content can be converted into biochar in the subsequent second roasting process, thereby further increasing the porosity and adsorption performance of the adsorbent.

[0030] Preferably, in S4, the voltage of the power-on pressurization is 5V~8V, and the time of the power-on pressurization is 1h~1.5h.

[0031] The present invention can better embed iron ions and coconut shell powder into the graphite block material by limiting the conditions of power-on and pressure-on.

[0032] For example, in S4, after the power-on and pressurization, the graphite block material after the power-on and pressurization needs to be dried and made neutral.

[0033] Preferably, in S5, the temperature of the second calcination is 500° C. to 600° C., and the time is 3 h to 3.5 h.

[0034] Preferably, in S5, the particle size of the iron-carrying biochar adsorbent is 100 nm to 800 nm, and the pore volume is 1.2 cm 3 / g~1.6cm 3 / g.

[0035] In a second aspect, the present invention provides an iron-loaded biochar adsorbent, which is prepared by the preparation method of the iron-loaded biochar adsorbent.

[0036] The iron-loaded biochar adsorbent provided by the present invention has a large adsorption capacity and good selectivity for phosphorus and heavy metals in sewage, which can further improve the adsorption efficiency of sewage treatment. The results of the embodiment show that after adsorption by the iron-loaded biochar adsorbent provided by the present invention, PO4 3- The removal rate can reach over 98%, and the adsorption capacity can reach over 49 mg / g.

[0037] In a third aspect, the present invention provides an iron-loaded biochar adsorbent prepared by the method for preparing the iron-loaded biochar adsorbent or the use of the iron-loaded biochar adsorbent in sewage treatment. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0039] Example 1 This embodiment provides a method for preparing an iron-loaded biochar adsorbent, comprising the following steps: S1, add the crushed biomass (plant straw) into an acid solution with a pH of 2-4, the mass volume ratio of biomass to acid solution is 1 g:8 mL, soak at room temperature for 7.5 hours, filter, wash the solid with hot water until it is neutral, and obtain a carbon source.

[0040] S2, heating the carbon source to 1050°C at a rate of 35°C / min, performing a first calcination for 2.5h, and grinding to obtain a graphitized carbon material.

[0041] S3, mixing graphitized carbon material, polyvinyl alcohol and water, wherein the mass ratio of graphitized carbon material, polyvinyl alcohol and water is 100:4:1.3; pressing at 70° C. and 27 MPa to obtain a graphite block material.

[0042] S4, using the graphite block material as the negative electrode, and placing it together with the platinum electrode (positive electrode) in a soluble iron salt solution, adding coconut shell powder with a particle size of 7μm~8μm, the mass ratio of the graphite block material to the coconut shell powder is 100:15, and after applying power and pressure (6V) for 1.5h, the graphite block material after power and pressure is dried and water-soluble to neutral to obtain a biochar precursor material.

[0043] The soluble iron salt solution contains FeSO4·7H2O and FeCl3·6H2O, Fe 2+ The concentration of Fe is 0.2 mol / L. 3+ The concentration is 0.3 mol / L; the pH of the soluble iron salt solution is 5.5.

[0044] S5, the biochar precursor material was second calcined at 550 °C for 3.5 h and ground to obtain a particle size of 400 nm to 500 nm and a pore volume of 1.4 cm 3 / g~1.5cm 3 / g of iron-loaded biochar adsorbent.

[0045] Example 2 This embodiment provides a method for preparing an iron-loaded biochar adsorbent, comprising the following steps: S1, adding the crushed biomass (branches) into an acid solution with a pH value of 2, the mass volume ratio of the biomass to the acid solution is 1 g:6 mL, soaking at room temperature for 7 hours, filtering, and washing the solid with hot water until it is neutral to obtain a carbon source.

[0046] S2, heating the carbon source to 1000°C at a rate of 30°C / min, performing a first calcination for 3h, and grinding to obtain a graphitized carbon material.

[0047] S3, mixing graphitized carbon material, polyvinyl alcohol and water, wherein the mass ratio of graphitized carbon material, polyvinyl alcohol and water is 100:3:1.5; pressing at 80° C. and 25 MPa to obtain a graphite block material.

[0048] S4, using the graphite block material as the negative electrode, and placing it together with the platinum electrode (positive electrode) in a soluble iron salt solution, adding coconut shell powder with a particle size of 5μm~6μm, the mass ratio of the graphite block material to the coconut shell powder is 100:10, and after applying power and pressure (5V) for 1.5h, the graphite block material after power and pressure is dried and water-soluble to neutral to obtain a biochar precursor material.

[0049] The soluble iron salt solution contains FeSO4·7H2O and FeCl3·6H2O, Fe 2+ The concentration of Fe is 0.3 mol / L, 3+ The concentration is 0.4 mol / L; the pH of the soluble iron salt solution is 5.

[0050] S5, the biochar precursor material was second calcined at 500 °C for 3.5 h and ground to obtain a particle size of 100 nm to 300 nm and a pore volume of 1.5 cm 3 / g~1.6cm 3 / g of iron-loaded biochar adsorbent.

[0051] Example 3 This embodiment provides a method for preparing an iron-loaded biochar adsorbent, comprising the following steps: S1, add the crushed biomass (plant straw and waste wood in equal mass ratio) into an acid solution of pH=4, the mass volume ratio of biomass and acid solution is 1g:10mL, soak at room temperature for 8h, filter, wash the solid with hot water until neutral, and obtain the carbon source.

[0052] S2, heating the carbon source to 1100° C. at a rate of 40° C. / min, performing a first calcination for 2 h, and grinding to obtain a graphitized carbon material.

[0053] S3, mixing graphitized carbon material, polyvinyl alcohol and water, wherein the mass ratio of graphitized carbon material, polyvinyl alcohol and water is 100:5:1; and pressing at 60° C. and 30 MPa to obtain a graphite block material.

[0054] S4, using the graphite block material as the negative electrode, and placing it together with the platinum electrode (positive electrode) in a soluble iron salt solution, adding coconut shell powder with a particle size of 9μm~10μm, the mass ratio of the graphite block material to the coconut shell powder is 100:20, and after applying power and pressure (8V) for 1h, the graphite block material after power and pressure is dried and water-soluble to neutral to obtain a biochar precursor material.

[0055] The soluble iron salt solution contains FeSO4·7H2O and FeCl3·6H2O, Fe 2+ The concentration of Fe is 0.3 mol / L, 3+ The concentration is 0.4 mol / L; the pH of the soluble iron salt solution is 5.

[0056] S5, the biochar precursor material was second calcined at 600 °C for 3 h and ground to obtain a particle size of 700 nm to 800 nm and a pore volume of 1.2 cm 3 / g~1.3cm 3 / g of iron-loaded biochar adsorbent.

[0057] Example 4 This embodiment provides a method for preparing an iron-loaded biochar adsorbent, comprising the following steps: S1, add the crushed biomass (twigs and flowers in equal mass ratio) into an acid solution with pH=3, the mass volume ratio of biomass and acid solution is 1g:8mL, soak at room temperature for 7.5h, filter, wash the solid with hot water until neutral, and obtain the carbon source.

[0058] S2, heating the carbon source to 1050°C at a rate of 35°C / min, performing a first calcination for 2.5h, and grinding to obtain a graphitized carbon material.

[0059] S3, mixing graphitized carbon material, polyvinyl alcohol and water, wherein the mass ratio of graphitized carbon material, polyvinyl alcohol and water is 100:4:1.3; pressing at 70° C. and 28 MPa to obtain a graphite block material.

[0060] S4, using the graphite block material as the negative electrode, and placing it together with the platinum electrode (positive electrode) in a soluble iron salt solution, adding coconut shell powder with a particle size of 8μm~9μm, the mass ratio of the graphite block material to the coconut shell powder is 100:15, and after applying power and pressure (7V) for 1.5h, the graphite block material after power and pressure is dried and water-soluble to neutral to obtain a biochar precursor material.

[0061] The soluble iron salt solution contains FeSO4·7H2O and FeCl3·6H2O, Fe 2+ The concentration of Fe is 0.3 mol / L, 3+ The concentration is 0.3 mol / L; the pH of the soluble iron salt solution is 5.5.

[0062] S5, the biochar precursor material was second calcined at 550 °C for 3 h and ground to obtain a particle size of 300 nm to 400 nm and a pore volume of 1.3 cm 3 / g~1.4cm 3 / g of iron-loaded biochar adsorbent.

[0063] Comparative Example 1 This comparative example provides a method for preparing an iron-carrying biochar adsorbent, which is similar to Example 1, except that in S2, the heating rate is 10°C / min. The other conditions are the same as those in Example 1 and will not be described in detail. The final particle size is 400nm~500nm and the pore volume is 1.0cm 3 / g~1.1cm 3 / g of iron-loaded biochar adsorbent.

[0064] Comparative Example 2 This comparative example provides a method for preparing an iron-carrying biochar adsorbent, which is similar to Example 1, except that in S2, the heating rate is 60°C / min. The other conditions are the same as those in Example 1 and will not be described in detail. The final particle size is 400nm~500nm and the pore volume is 0.9cm 3 / g~1.0cm 3 / g of iron-loaded biochar adsorbent.

[0065] Comparative Example 3 This comparative example provides a method for preparing an iron-carrying biochar adsorbent, which is similar to Example 1, except that in S2, the temperature of the first calcination is 800°C. The remaining conditions are the same as those in Example 1 and will not be described in detail. The final particle size is 500nm~600nm and the pore volume is 0.9cm 3 / g~1.0cm 3 / g of iron-loaded biochar adsorbent.

[0066] Comparative Example 4 This comparative example provides a method for preparing an iron-loaded biochar adsorbent, which is similar to Example 1, except that: in S3, the addition of polyvinyl alcohol is omitted. The remaining conditions are the same as those in Example 1 and will not be repeated. The final particle size is 400nm~500nm and the pore volume is 1.4cm 3 / g~1.5cm 3 / g of iron-loaded biochar adsorbent.

[0067] Comparative Example 5 This comparative example provides a method for preparing an iron-loaded biochar adsorbent, comprising the following steps: S1~S3 are the same as those in Example 1 and will not be described in detail.

[0068] S4, adding the graphite block material to a soluble iron salt solution, adding coconut shell powder with a particle size of 7μm~8μm, the mass ratio of the graphite block material to the coconut shell powder is 100:15, stirring and impregnating for 8 hours, drying the impregnated graphite block material, and water-based to neutral, to obtain a biochar precursor material.

[0069] The soluble iron salt solution contains FeSO4·7H2O and FeCl3·6H2O, Fe2+ The concentration of Fe is 0.2 mol / L. 3+ The concentration is 0.3 mol / L; the pH of the soluble iron salt solution is 5.5.

[0070] S5, same as Example 1, no further description is given. The final particle size is 700nm~800nm ​​and the pore volume is 0.8cm 3 / g~0.9cm 3 / g of iron-loaded biochar adsorbent.

[0071] Comparative Example 6 This comparative example provides a method for preparing an iron-loaded biochar adsorbent, which is similar to Example 1, except that in S4, coconut shell powder is omitted. The remaining conditions are the same as those in Example 1 and are not described in detail. The final particle size is 400nm~500nm and the pore volume is 1.3cm 3 / g~1.4cm 3 / g of iron-loaded biochar adsorbent.

[0072] Comparative Example 7 This comparative example provides a method for preparing an iron-carrying biochar adsorbent, which is similar to Example 1, except that: in S4, the soluble iron salt solution contains only divalent iron salt FeSO4·7H2O, Fe 2+ The concentration of is 0.2 mol / L. The other conditions are the same as those in Example 1 and will not be repeated here. The final particle size is 400 nm to 500 nm and the pore volume is 1.4 cm 3 / g~1.5cm 3 / g of iron-loaded biochar adsorbent.

[0073] Comparative Example 8 This comparative example provides a method for preparing an iron-carrying biochar adsorbent, which is similar to Example 1, except that: in S4, the soluble iron salt solution contains only trivalent iron salt FeCl3·6H2O, Fe 3+ The concentration of is 0.3 mol / L. The other conditions are the same as those in Example 1 and will not be repeated here. The final particle size is 400 nm to 500 nm and the pore volume is 1.4 cm 3 / g~1.5cm 3 / g of iron-loaded biochar adsorbent.

[0074] Comparative Example 9 This comparative example provides a method for preparing an iron-loaded biochar adsorbent, comprising the following steps: S1~S2 are the same as those in Example 1 and will not be described in detail.

[0075] S3, adding the graphitized carbon material into a soluble iron salt solution, stirring and impregnating for 8 hours, drying the impregnated graphitized carbon material, and aqueous to neutral to obtain a biochar precursor material.

[0076] The soluble iron salt solution contains FeSO4·7H2O and FeCl3·6H2O, Fe 2+ The concentration of Fe is 0.2 mol / L. 3+ The concentration is 0.3 mol / L; the pH of the soluble iron salt solution is 5.5.

[0077] S4 is the same as S5 in Example 1 and will not be described in detail. The final particle size is 700nm-800nm ​​and the pore volume is 0.8cm 3 / g~0.9cm 3 / g of iron-loaded biochar adsorbent.

[0078] Verification test In order to verify the phosphorus removal effect of the iron-loaded biochar adsorbent provided in Examples 1 to 4 and Comparative Examples 1 to 9 on sewage, the following test was conducted: high-grade pure potassium dihydrogen phosphate was dried at 110°C for 2h, cooled in a dryer, and 13 portions of phosphorus-containing wastewater (in terms of P) with a concentration of 100mg / L were prepared, each with 1L as simulated sewage; 2g of the iron-loaded biochar adsorbent of the embodiments and comparative examples were taken, respectively, and put into 13 portions of simulated sewage, and put into an oscillator, and the temperature was set to 25°C, the speed was 150rpm, and the oscillation was performed for 30min. Then, membrane filtration was used, and the phosphorus content in the filtrate was determined by molybdenum antimony anti-spectrophotometry, and the adsorption amount of the adsorbent was calculated. The specific results are shown in Table 1.

[0079] Table 1 Comparison of phosphorus removal effects of adsorbents on sewage

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an iron-loaded biochar adsorbent, characterized in that: The following steps are involved: S1, adding biomass into an acid solution for impregnation to obtain a carbon source; S2, heating the carbon source to 1000° C. to 1100° C. at a rate of 30° C. / min to 40° C. / min for a first calcination to obtain a graphitized carbon material; S3, mixing the graphitized carbon material, polyvinyl alcohol and water, and pressing to obtain a graphite block material; S4, placing the graphite block material as one end of an electrode together with a platinum electrode into a soluble iron salt solution, adding coconut shell powder, and applying electricity and pressure to obtain a biochar precursor material; The soluble iron salt solution includes divalent iron salt and trivalent iron salt; S5, performing a second calcination on the biochar precursor material, and crushing the biochar precursor material to obtain an iron-loaded biochar adsorbent.

2. The method for preparing the iron-loaded biochar adsorbent according to claim 1, characterized in that: In S1, the biomass is selected from plant straw, branches, waste wood or flowers and plants; and / or In S1, the pH of the acid solution is 2-4; and / or In S1, the mass volume ratio of the biomass to the acid solution is 1 g: (6-10) mL.

3. The method for preparing the iron-loaded biochar adsorbent according to claim 1, characterized in that: In S1, the immersion temperature is 5°C to 40°C, and the immersion time is 7h to 8h; and / or In S2, the first calcination time is 2h~3h.

4. The method for preparing the iron-loaded biochar adsorbent according to claim 1, characterized in that: In S3, the mass ratio of the graphitized carbon material, the polyvinyl alcohol and the water is 100:(3-5):(1-1.5); and / or In S3, the pressing temperature is 60° C. to 80° C., the pressing pressure is 25 MPa to 30 MPa, and the holding time is 3 s to 4 s.

5. The method for preparing the iron-loaded biochar adsorbent according to claim 1, characterized in that: In S4, the concentration of the divalent iron salt in the soluble iron salt solution is 0.2 mol / L to 0.3 mol / L, and the concentration of the trivalent iron salt is 0.3 mol / L to 0.4 mol / L; and / or In S4, the divalent iron salt is ferrous sulfate, and the trivalent iron salt is ferric chloride; and / or In S4, the pH of the soluble iron salt solution is 5-5.

5.

6. The method for preparing the iron-loaded biochar adsorbent according to claim 1, characterized in that: In S4, the particle size of the coconut shell powder is 5 μm to 10 μm; and / or In S4, the mass ratio of the graphite block material to the coconut shell powder is 100:(10-20).

7. The method for preparing the iron-loaded biochar adsorbent according to claim 1, characterized in that: In S4, the voltage of the power-on and pressurization is 5V to 8V, and the time of the power-on and pressurization is 1h to 1.5h; and / or In S5, the second calcination is performed at a temperature of 500°C to 600°C and for a time of 3h to 3.5h.

8. The method for preparing the iron-loaded biochar adsorbent according to claim 1, characterized in that: In S5, the particle size of the iron-carrying biochar adsorbent is 100 nm to 800 nm, and the pore volume is 1.2 cm 3 / g~1.6cm 3 / g.

9. An iron-carrying biochar adsorbent, characterized in that: The biochar adsorbent is prepared by the method for preparing the iron-loaded biochar adsorbent according to any one of claims 1 to 8.

10. Use of the iron-loaded biochar adsorbent prepared by the preparation method of the iron-loaded biochar adsorbent according to any one of claims 1 to 8 or the iron-loaded biochar adsorbent according to claim 9 in sewage treatment.