Defective Cu-Mo co-doped Mn0. 5Cd0. 5S composite photocatalyst and application thereof in photocatalysis
By introducing sulfur vacant positions on the Mn0.5Cd0.5S surface and using bimetal doping of Cu and Mo, a defective Cu-Mo co-doped Mn0.5Cd0.5S catalyst was formed, and the problem of low efficiency of MnxCd1-xS photocatalyst was solved. The performance and stability of H2O2 preparation are significantly improved.
Patent Information
- Application Number
- CN202411017219.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-26
AI Technical Summary
MnxCd1-xS photocatalyst is not efficient in photocatalytic oxygen reduction reactions, and the single defect or metal doping modification effect is limited, making it difficult to effectively improve its performance in photocatalytic preparation of H2O2.
By introducing sulfur vacancy on the surface of Mn0.5Cd0.5S and using bimetal doping of Cu and Mo, a defective Cu-Mo co-doped Mn0.5Cd0.5S composite catalyst is formed, and the light absorption range and metal ions are expanded using sulfur vacancy. Complementary action improves carrier separation efficiency.
The activity of the photocatalyst under visible light and the precipitation performance of H2O2 in a significantly improved manner, and the rate and stability of photocatalytic preparation of H2O2 are improved.
Smart Images

Figure CN118925752A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of inorganic materials, and specifically relates to defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S composite catalyst and its application in photocatalysis. Background Art
[0002] As a green and multifunctional chemical raw material, hydrogen peroxide (H2O2) has strong oxidizing ability and is widely used in medicine, textiles, energy and other fields. Compared with the anthraquinone oxidation method, which consumes a lot of energy and has complicated processes, the photocatalytic oxygen reduction reaction (ORR) technology can use abundant solar energy to reduce dissolved oxygen in water into H2O2 through photogenerated electrons on the photocatalyst. Among the many catalysts for photocatalytic production of H2O2, Mn x Cd 1-x As a low-cost and readily available sulfur solid solution photocatalyst, S shows excellent potential in photocatalytic H2O2 production due to its suitable band gap structure and controllability. x Cd 1-x The rapid recombination of photogenerated carriers and the lack of active sites in S make the efficiency of photocatalytic production of H2O2 by reducing O2 in water not optimistic. x Cd 1-x In order to improve the photocatalytic hydrogen production performance of S materials, people have adopted a variety of strategies to modify them, such as defect regulation, metal doping, composite with semiconductor materials, and loading of different co-catalysts.
[0003] Defect engineering is considered to increase Mn x Cd 1-x S catalysts are an effective strategy for the utilization rate of photogenerated carriers and light absorption rate, and some studies have also proved this point of view. x Cd 1-x The introduction of surface vacancies or defects formed by surface functional groups in S photocatalysts will provide more capture sites, promoting electron accumulation and carrier separation. x Cd 1-x S materials play a role in promoting the photocatalytic activity, but a single type of defect has an x Cd 1-x The performance of S materials in photocatalytic preparation of H2O2 is limited. x Cd 1-x The capture centers of electrons and holes are formed on the surface of S, thereby inhibiting the recombination of photogenerated electrons and holes. In addition, the doping of transition metal ions can also x Cd 1-xCompared with single metal doping, double metal doping can utilize the complementary effect between two metal ions to make Mn x Cd 1-x S has a wider light absorption range and higher carrier separation efficiency.
[0004] The present invention uses Mn 0.5 Cd 0.5 S nanowires as the main catalyst, and defective Cu-Mo co-doped Mn was successfully prepared by a simple one-step hot solvent method. 0.5 Cd 0.5 S composite catalyst and applied it to the photocatalytic preparation of H2O2. 0.5 Cd 0.5 The introduction of sulfur vacancies on the S surface can not only expand the light absorption range of the catalyst, but also effectively promote the separation and transmission of photogenerated carriers, thereby improving the Mn 0.5 Cd 0.5 S has photocatalytic activity under visible light. The dual doping of transition metal ions Cu and Mo can utilize the complementary effect between the two metal ions to make Mn 0.5 Cd 0.5 S has a wider light absorption range and higher carrier separation efficiency. Based on the above advantages, the defective Cu-Mo co-doped Mn 0.5 Cd 0.5 The S composite catalyst has shown good application in the photocatalytic preparation of H2O2. Summary of the invention
[0005] The present invention provides a defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S composite catalyst and its preparation method and its application in photocatalytic production of H2O2, the defective Cu-Mo co-doped Mn 0.5 Cd 0.5 The S composite catalyst has the advantages of high photocatalytic activity for preparing H2O2 and stable performance.
[0006] The defective Cu-Mo co-doped Mn 0.5 Cd 0.5 The structural characteristics of S composite catalyst are as follows: 0.5 Cd 0.5 There are sulfur vacancies on the S surface; Mn 0.5 Cd 0.5The molar ratio of S, Cu and Mo is 1:0.01-0.1:0.01-0.1; there are strong diffraction peaks at 25.4°, 27.2°, 28.9°, 37.5°, 44.6°, 49.4° and 53.0° in the XRD spectrum; there are binding energies at 160.8eV, 162.1eV, 404.4eV, 411.2eV, 640.8eV, 652.7eV, 932.9eV, 952.7eV, 224.9eV and 225.6eV in the XPS spectrum; there is a signal peak of sulfur defect at g=2.004 in the paramagnetic resonance spectrum; defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S is a nanowire structure.
[0007] from Figure 1 It can be clearly observed in the XRD sample crystal structure: Mn 0.5 Cd 0.5 The S sample has strong diffraction peaks at 25.4°, 27.2°, 28.9°, 37.5°, 44.6°, 49.4° and 53.0°, which are consistent with the Mn 0.5 Cd 0.5 S XRD standard spectrum is consistent. In addition, Cu doped or Cu-Mo co-doped Mn 0.5 Cd 0.5 No Cu or Mo compounds were observed in the S XRD pattern, indicating that no new substances were formed by the doping of Cu and Mo.
[0008] from Figure 2 XPS Analysis of Defective Cu-Mo Co-doped Mn 0.5 Cd 0.5 The elemental composition spectrum of the S sample shows that: Mn 2p 3 / 2 and Mn 2p 1 / 2 The binding energies are 640.8eV and 652.7eV; Cd 3d 5 / 2 and Cd 3d 3 / 2 The binding energies are 404.4eV and 411.2eV; S2p 3 / 2 and S2p 1 / 2 The binding energy is between 160.8eV and 162.1eV; Cu 2p 3 / 2 and Cu 2p 1 / 2 The binding energies are 932.9eV and 952.7eV, and the 225.6eV binding energy is attributed to the Mo-S bond. In addition, it can be seen from the XPS overall spectrum that the five elements S, Mn, Cd, Cu and Mo exist at the same time, and no peaks of other impurities are detected, indicating that high-purity Cu-Mo co-doped Mn 0.5 Cd 0.5 S complex.
[0009] from Figure 3 From the TEM and SEM sample morphology, it can be seen that Cu-Mo co-doped Mn 0.5 Cd 0.5 The S sample exhibits a regular nanowire structure with a wire length of about 2 μm and a diameter of about 50 nm.
[0010] from Figure 4 It can be seen from the UV-visible diffuse reflectance spectrum that Cu-Mo co-doped Mn 0.5 Cd 0.5 The absorption band edge of the S sample is red-shifted, and the absorption performance in the visible light region is significantly stronger than that of undoped Mn 0.5 Cd 0.5 S, indicating that bimetallic doping can further optimize the light absorption properties of the composite catalyst.
[0011] from Figure 5 It can be seen from the transient photocurrent spectrum that Mn 0.5 Cd 0.5 S exhibits a lower current density, indicating that only a small amount of photogenerated electrons participate in the transfer and separation process; compared with Mn 0.5 Cd 0.5 Compared with S, Cu-doped Cu-Mn 0.5 Cd 0.5 S transient photocurrent intensity increases significantly, Cu-Mo co-doped Mn 0.5 Cd 0.5 The S current intensity is the highest, which further proves that bimetallic doping can further accelerate the separation of photogenerated electrons and holes.
[0012] from Figure 6 It can be seen from the electrochemical impedance spectrum that the Nyquist radius is in the following order: Mn 0.5 Cd 0.5 S>Cu-Mn 0.5 Cd 0.5 S>Mo / Cu-Mn 0.5 Cd 0.5 S, indicating that Cu-Mo co-doping can effectively reduce the interface charge transfer resistance and improve the photocatalytic performance of H2O2 production.
[0013] from Figure 7 The paramagnetic resonance spectrum shows that there is an obvious signal peak at g = 2.004, indicating that the prepared Cu-Mo co-doped Mn 0.5 Cd 0.5 There are S vacancies on the S surface.
[0014] from Figure 8 The photocatalytic H2O2 production experiment shows that pure Mn 0.5 Cd 0.5 S exhibits poor H2O2 performance due to rapid charge carrier recombination; after Cu doping, the resulting Cu-Mn0.5 Cd 0.5 The performance of H2O2 evolution of S composite photocatalyst is improved; when Cu and Mo are doped into Mn 0.5 Cd 0.5 Cu-Mo co-doped with Mn 0.5 Cd 0.5 The S composite photocatalyst has the highest performance in H2O2 evolution, indicating that the synergistic effect of bimetallic doping can greatly enhance the performance of Mn 0.5 Cd 0.5 S analysis of H2O2 performance.
[0015] The defective Cu-Mo co-doped Mn 0.5 Cd 0.5 The preparation method of the S composite catalyst is characterized by comprising the following steps:
[0016] 1) dissolving cadmium acetate, manganese acetate, thioacetamide and copper nitrate in ethylenediamine solution, and then stirring the solution evenly at room temperature;
[0017] Furthermore, in the above technical solution, the molar ratio of manganese acetate to cadmium acetate is 1:1; the molar ratio of manganese acetate to thioacetamide is 1:2-4; and the molar ratio of manganese acetate to copper nitrate is 1:0.02-0.2.
[0018] 2) Sodium molybdate is added to the above ethylenediamine solution, and the resulting mixed solution is subjected to a hot solvent reaction at 140-200°C after continued stirring to obtain defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S nanowires.
[0019] Furthermore, in the above technical solution, the molar ratio of manganese acetate to sodium molybdate is 1:0.02-0.2.
[0020] The defective Cu-Mo co-doped Mn 0.5 Cd 0.5 Application of S composite catalyst in photocatalytic production of H2O2.
[0021] Furthermore, in the above technical solution, the photocatalytic reaction operating conditions are: light source 300W xenon lamp; catalyst amount 100mg; deionized water amount 90mL; isopropanol amount 10mL. Preparation of H2O2 from photocatalysis Figure 8 It can be seen that pure Mn 0.5 Cd 0.5 The photocatalytic rate of S to produce H2O2 was 0.83 mmol g -1 h -1 , Cu doped Mn 0.5 Cd 0.5 The photocatalytic rate of S to produce H2O2 was 2.86 mmol g-1 h -1 , Cu and Mo co-doped Mn 0.5 Cd 0.5 The photocatalytic rate of S to produce H2O2 was 5.37 mmol g -1 h -1 , showing significantly enhanced photocatalytic H2O2 production performance. Beneficial effects of the present invention:
[0022] The defective Cu-Mo co-doped Mn 0.5 Cd 0.5 The S composite catalyst is a nanowire structure, in which Mn 0.5 Cd 0.5 The introduction of sulfur vacancies on the S surface can not only expand the light absorption range of the catalyst, but also effectively promote the separation and transmission of photogenerated carriers, thereby improving the Mn 0.5 Cd 0.5 S photocatalytic activity under visible light. The dual doping of transition metal ions Cu and Mo can utilize the complementary effect between the two metal ions to make Mn 0.5 Cd 0.5 S has a wider light absorption range and higher carrier separation efficiency, which makes the defective Cu-Mo co-doped Mn 0.5 Cd 0.5 The H2O2 precipitation performance of S composite photocatalyst is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S, Cu doped Mn 0.5 Cd 0.5 S and Cu-Mo co-doped Mn 0.5 Cd 0.5 S XRD pattern;
[0024] Figure 2 The defective Cu-Mo co-doped Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S XPS spectrum;
[0025] Figure 3 The defective Cu-Mo co-doped Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S SEM image (a) and TEM image (b);
[0026] Figure 4 Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S, Cu doped Mn 0.5 Cd0.5 S and Cu-Mo co-doped Mn 0.5 Cd 0.5 S UV-Vis diffuse reflectance spectrum.
[0027] Figure 5 Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S, Cu doped Mn 0.5 Cd 0.5 S and Cu-Mo co-doped Mn 0.5 Cd 0.5 S transient current spectrum;
[0028] Figure 6 Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S, Cu doped Mn 0.5 Cd 0.5 S and Cu-Mo co-doped Mn 0.5 Cd 0.5 S electrochemical impedance spectroscopy;
[0029] Figure 7 The defective Cu-Mo co-doped Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S solid state paramagnetic resonance spectrum.
[0030] Figure 8 Mn prepared in Example 1 of the present invention 0.5 Cd 0.5 S, Cu doped Mn 0.5 Cd 0.5 S and Cu-Mo co-doped Mn 0.5 Cd 0.5 S Photocatalytic H2O2 production effect diagram; DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the embodiments. It should be noted that the present invention is not limited to the following embodiments.
[0032] Example 1
[0033] 1) Dissolve 0.9391 g of thioacetamide, 0.9926 g of manganese acetate tetrahydrate, 1.1994 g of cadmium acetate dihydrate and 0.1087 g of copper nitrate trihydrate in 60 mL of ethylenediamine, and stir vigorously at room temperature for 30 min to make it uniform;
[0034] 2) Add 0.1318 g of sodium molybdate dihydrate to the above ethylenediamine solution, continue stirring for 30 min, transfer the mixed solution to a 100 mL Teflon-lined stainless steel autoclave, and keep it at 160 ° C for 24 hours. The obtained sample is centrifuged, washed, and dried to obtain defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S composite photocatalyst.
[0035] Example 2
[0036] 1) Dissolve 0.7513 g of thioacetamide, 0.9926 g of manganese acetate tetrahydrate, 1.1994 g of cadmium acetate dihydrate and 0.0217 g of copper nitrate trihydrate in 60 mL of ethylenediamine, and stir vigorously at room temperature for 30 min to make it uniform;
[0037] 2) Add 0.0264 g of sodium molybdate dihydrate to the above ethylenediamine solution, continue stirring for 30 min, transfer the mixed solution to a 100 mL Teflon-lined stainless steel autoclave, and keep it at 140 ° C for 24 hours. The obtained sample is centrifuged, washed, and dried to obtain defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S composite photocatalyst.
[0038] Example 3
[0039] 1) Dissolve 1.5026 g of thioacetamide, 0.9926 g of manganese acetate tetrahydrate, 1.1994 g of cadmium acetate dihydrate and 0.2174 g of copper nitrate trihydrate in 60 mL of ethylenediamine, and stir vigorously at room temperature for 30 min to make it uniform;
[0040] 2) 0.2636 g of sodium molybdate dihydrate was added to the above ethylenediamine solution, and the mixture was transferred to a 100 mL Teflon-lined stainless steel autoclave after stirring for 30 min, and kept at 200 ° C for 24 hours. The obtained sample was centrifuged, washed, and dried to obtain defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S composite photocatalyst.
[0041] Example 4 Photocatalytic H2O2 production experiment:
[0042] 100 mg of the catalyst was evenly dispersed in a mixed solution containing 10 mL of isopropanol and 90 mL of water. After ultrasonic treatment for 10 min, oxygen was continuously introduced and stirred for 30 min in the dark. A 300 W xenon lamp was used as the light source for the photocatalytic H2O2 production experiment. Figure 8 It can be seen that pure Mn 0.5 Cd 0.5The photocatalytic H2O2 evolution rate of S was 0.83 mmol g -1 h -1 , using the Cu-doped Mn obtained in Example 1 0.5 Cd 0.5 The photocatalytic H2O2 evolution rate of S was 2.86 mmol g -1 h -1 , and the Cu-Mo co-doped Mn obtained in Example 1 is used 0.5 Cd 0.5 The photocatalytic H2O2 evolution rate of S was as high as 5.37 mmol g -1 h -1 , showing significantly enhanced photocatalytic H2O2 evolution performance.
[0043] The composite photocatalyst prepared by using Example 2-3 can obtain a similar effect of producing hydrogen peroxide.
[0044] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. Defective Cu-Mo co-doped with Mn 0.5 Cd 0.5 S composite catalyst, characterized by: Mn in composite catalyst 0.5 Cd 0.5 There are sulfur vacancies on the S surface; Mn 0.5 Cd 0.5 The molar ratio of S, Cu and Mo is 1:0.01-0.1:0.01-0.1; there are strong diffraction peaks at 25.4°, 27.2°, 28.9°, 37.5°, 44.6°, 49.4° and 53.0° in the XRD spectrum; there are binding energies at 160.8eV, 162.1eV, 404.4eV, 411.2eV, 640.8eV, 652.7eV, 932.9eV, 952.7eV, 224.9eV and 225.6eV in the XPS spectrum; there is a signal peak of sulfur defect at g=2.004 in the paramagnetic resonance spectrum; defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S is a nanowire structure.
2. Defective Cu-Mo co-doped Mn as claimed in claim 1 0.5 Cd 0.5 The method for preparing the S composite catalyst is characterized in that: The steps include: 1) dissolving cadmium acetate, manganese acetate, thioacetamide and copper nitrate in ethylenediamine solution, and then stirring the solution evenly at room temperature; 2) Sodium molybdate is added to the above ethylenediamine solution, and the resulting mixed solution is subjected to a hot solvent reaction at 140-200°C after continued stirring to obtain defective Cu-Mo co-doped Mn 0.5 Cd 0.5 S composite catalyst.
3. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 1), the molar ratio of manganese acetate to cadmium acetate is 1:
1.
4. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 1), the molar ratio of manganese acetate to thioacetamide is 1:2-4.
5. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 1), the molar ratio of manganese acetate to copper nitrate is 1:0.02-0.
2.
6. The method for preparing the composite photocatalyst according to claim 2, characterized in that: The molar ratio of manganese acetate in step 1) to sodium molybdate in step 2) is 1:0.02-0.
2.
7. Defective Cu-Mo co-doped Mn as claimed in claim 1 0.5 Cd 0.5 Application of S composite catalyst in photocatalytic preparation of H2O2.
8. The defective Cu-Mo co-doped Mn according to claim 7 0.5 Cd 0.5 The application of S composite catalyst in photocatalytic preparation of H2O2 is characterized by: The operating conditions are: light source 300W xenon lamp; catalyst amount 100mg; deionized water amount 90mL; isopropanol amount 10mL.
Citation Information
Patent Citations
Method for preparing molybdyl modified quaternary sulfide quantum dot photocatalyst
CN107243349A
Hierarchy MoS2 / Cu2S composite material and preparation method thereof
CN107262116A
Application of transition metal sulfide Mn-Cd-S-loaded solid solution in photocatalysis hydrogen production aspect
CN107376944A
Preparation method of supported photocatalyst containing Mn0.5Cd0.5S and Cu2O
CN110586135A
Preparation method and application of transition metal molybdate heterojunction photocatalytic material
CN115364871A