Preparation method of catalytic cracking catalyst with low coke yield and high gasoline and diesel oil yield

By modifying the Elosite, calcined kaolin, alumina and Y-type molecular sieve, combined with acidic liquid, a catalyst with low coke and high coke production is formed, and the catalyst with low catalyst conversion rate and high coke production in the prior art is solved. The problem has achieved more efficient gasoline and diesel conversion and catalyst performance improvement.

CN118925784APending Publication Date: 2024-11-12QINGDAO HUICHENG PETROCHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410993503.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing FCC catalysts have low conversion rate, high coking yield when treating heavy crude oil, high cost, small acid ratio, poor synergistic effect between matrix and molecular sieve, making it difficult to achieve the goal of low coking and high yield of gasoline and diesel.

Method used

The medium-strong acid position is formed by using eloite and modifier treatment, calcined kaolin forms a large pore size, alumina is combined with silicon-aluminum matrix material, Y-type molecular sieve is subjected to rare earth ion exchange and hydrothermal treatment, combined with acid liquid for spray granulation and roasting, and is adjusted The pH value and acidic center form a catalyst for low-growth coke and high-yield gasoline and diesel.

Benefits of technology

It significantly improves the pre-cracking depth and diffusion ability of the catalyst to heavy oil macromolecules, reduces coking production, improves the conversion rate of gasoline and diesel and the accessibility of the acidic center of the catalyst, and meets the demand for gasoline and diesel production with low coking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959503350000041
    Figure BDA0004959503350000041
  • Figure BDA0004959503350000042
    Figure BDA0004959503350000042
Patent Text Reader

Abstract

The invention relates to a preparation method of a catalytic cracking catalyst with low green coke and high gasoline and diesel yield, and solves the contradiction between high gasoline and diesel yield and green coke in a refinery plant. The method comprises the following steps: separately treating halloysite, calcined kaolin and an aluminum oxide material, then mixing with a Y-type molecular sieve, and carrying out spray granulation, so that the prepared catalyst has a matrix with gradient pore size distribution, the acidity and the acid amount are regulated and controlled, and the catalyst has a synergistic effect with the specially treated Y-type molecular sieve. When the catalyst is used in a refinery plant, more gasoline and diesel components with high added values can be obtained, green coke can be reduced, and higher economic benefits can be obtained for the refinery plant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a catalytic cracking catalyst with low coke generation and high gasoline and diesel production, belonging to the field of oil refining catalysts. Background Art

[0002] As oil resources decrease and crude oil becomes increasingly heavy, FCC, as the main means of converting heavy oil into gasoline and diesel, has a lower conversion rate and increased coke yield, and there are rigid requirements for reducing carbon emissions worldwide.

[0003] Coke is the product of hydrogen transfer reaction. Therefore, to improve coke production, it is necessary to control the hydrogen transfer reaction. In addition, it is also necessary to control the adsorption performance and molecular diffusion capacity of the catalyst.

[0004] CN103506153B discloses a catalytic cracking catalyst for reducing coke yield and producing gasoline, which contains 10-50% of modified Y-type molecular sieve on a dry basis, P is 0.05-6%, RE2O3 is 0.03-10%, and the hydroxyl nest concentration is less than 0.35mmol / g. The Y-type molecular sieve adopts a three-cross-baking and three-roasting process.

[0005] CN108786782B discloses a catalyst additive for reducing coke yield and a method thereof, which comprises a rare earth-containing medium- and macroporous silicon-aluminum material, an alumina material, a heavy metal collector and clay, and adopts cheap modified raw materials, and can significantly improve coke selectivity.

[0006] The commonly used active matrix of FCC catalyst is pseudo-boehmite, but its pore structure and acid strength can no longer meet the requirements of processing heavy crude oil.

[0007] CN104445317B discloses a method for preparing modified pseudo-boehmite.

[0008] CN03157163.8 discloses the synthesis of silica-alumina containing pseudo-boehmite structure.

[0009] Therefore, in order to achieve the goal of low coke production and high production of gasoline and diesel, researchers have carried out a lot of work, but there are still many shortcomings, such as the high cost of synthetic silicon-aluminum materials, small B / L acid ratio, and the inability of the matrix and molecular sieve to effectively cooperate. Summary of the invention

[0010] In view of the current shortcomings, the present invention provides a new preparation method that can significantly improve the shortcomings. The method comprises the following steps:

[0011] (1) Add halloysite to a rotary granulation device, slowly add a certain proportion of an aqueous solution containing a first modifier while the device is rotating, stir thoroughly, introduce hot air to raise the temperature of the material to 60-85° C., maintain for 10-50 minutes, then transfer the material to a reactor, add water to slurry, filter and wash, add water to slurry again, add a second modifier, and the slurry is recorded as A for standby use;

[0012] (2) calcined kaolin is slurried with water, and the third modifier is added to fully contact the slurry, which is recorded as B and set aside;

[0013] (3) Slurry A and B are mixed, a certain proportion of the fourth modifier is added, and the pH value is adjusted to 3.4-3.8. The slurry is recorded as C and is set aside;

[0014] (4) Alumina is slurried with water, solid content is controlled and pH value is adjusted to 1.8-2.5, and the slurry is kept for a period of time. The slurry is recorded as D and is set aside;

[0015] (5) Add a certain proportion of acidic liquid to the Y-type molecular sieve for full contact. The slurry is recorded as E and is set aside.

[0016] (6) Slurry C, slurry D and slurry E are added to a new reactor in sequence, mixed evenly, and then spray granulated, roasted, washed, filtered and dried to obtain a catalytic cracking catalyst with low coking and high gasoline and diesel production.

[0017] The first modifier is phosphoric acid, and the aqueous solution containing the first modifier is added in a ratio of (0.88-0.95)Pv·M, wherein Pv is the pore volume of halloysite, and M is the mass of halloysite. The concentration of the aqueous solution is 15-25wt% in terms of H3PO4.

[0018] The second modifier is silica sol, and the added ratio is 3-8wt% of the final catalyst dry weight calculated as SiO2.

[0019] The third modifier is hydrochloric acid.

[0020] The fourth modifier is calcium chloride or magnesium chloride, and the added ratio is 0.05-0.18 wt % of the final catalyst dry weight calculated as alkaline earth oxide.

[0021] The proportion of alumina added is 18-26 wt% of the final catalyst dry weight in terms of Al2O3, and the pore volume of alumina is 0.55-0.90 ml / g.

[0022] The Y-type molecular sieve has a unit cell constant of The NaY is subjected to rare earth ion exchange and hydrothermal treatment, and the non-framework aluminum content is controlled to be ≤4.6wt%, and the addition ratio accounts for 30-40wt% of the final catalyst dry weight.

[0023] The acidic liquid is formic acid or acetic acid, and the addition ratio is H + It is calculated as 0.0035-0.0045 of the Y-type molecular sieve dry basis.

[0024] The present invention is beneficial in that:

[0025] (1) After the halloysite is treated with the first modifier, part of the alumina combines with the modifier to form a hydroxyl site of a medium-strong acid, and then is treated with the fourth modifier to retain the appropriate number and strength of acid centers, which is beneficial to control the pre-cracking depth of heavy oil macromolecules and reduce coke formation;

[0026] (2) The calcined kaolin is treated with the third modifier to form a larger pore size and pore volume, which is conducive to the vaporization and diffusion of macromolecules. The aluminum removed and entering the solution can form a certain proportion of silicon-aluminum matrix material with the second modifier, further enhancing the cracking of heavy oil macromolecules;

[0027] (3) The role of the fourth modifier is to regulate the acid strength and acid density of the matrix, which is beneficial for the reaction products to separate from the acid center and diffuse in the catalyst, and is beneficial for reducing coke formation;

[0028] (4) Y-type molecular screening to obtain unit cell constants NaY is prone to produce more mesopores during hydrothermal treatment, and because there are more aluminum-oxygen tetrahedrons, it means there are more acidic centers, and the mesopores improve the accessibility of the acidic centers. DETAILED DESCRIPTION

[0029] The implementation of the present invention is described in detail below. It should be noted that this embodiment is not intended to limit the present invention, and the raw materials in the embodiments and comparative examples are all from the company's tank area or warehouse.

[0030] The analysis and evaluation are completed by our company's laboratory personnel.

[0031] Embodiment 1:

[0032] (1) 1181 g of halloysite (solid content 63.5%) was weighed and placed in a rotary granulator, 187 ml of the first modified liquid was added while the granulator was rotating, and hot air was introduced to raise the material temperature to 60-85° C. after thorough mixing, and the temperature was maintained for 35 minutes. The material was transferred to a reactor, 1500 g of water was added, and the material was slurried, washed, and filtered. After the filter cake was slurried again, 1333 g of silicon solution (30 wt%) was added, which was recorded as slurry A;

[0033] (2) Weigh 761 g of calcined kaolin (solid content 98.5%), add 1142 g of water to slurry, add hydrochloric acid to adjust the pH value, and keep for 30-90 minutes, which is recorded as slurry B;

[0034] (3) Slurries A and B were mixed evenly, 83.3 g of MgCl2 (MgO = 6%) was added, and the pH value was adjusted to 3.4-3.8, which was recorded as slurry C;

[0035] (4) Weigh 1692 g of alumina (ignition loss 35%) and add 2708 g of water, adjust the pH value to 1.8-2.5, and maintain for a period of time, which is recorded as slurry D;

[0036] (5) Weigh 6993 g of Y-type molecular sieve slurry (solid content 28.6%), add 1582.4 g of formic acid (25 wt %) solution, and record it as slurry E;

[0037] (6) Slurries C, D, and E are added to a new reactor in sequence, mixed evenly, and then spray granulated, filtered, washed, and dried. The collected catalyst is recorded as Cat-1.

[0038] Embodiment 2:

[0039] (1) Weighing 1299 g of halloysite (solid content 63.5%) and placing it in a rotary granulator, adding 187 ml of the first modified liquid while rotating, and passing hot air to raise the material temperature to 60-85° C. after thorough mixing, and maintaining it for 35 minutes, transferring the material to a reactor, adding 1500 g of water to slurry, and washing and filtering, after slurrying the filter cake again, adding 1000 g of silicon solution (30 wt %), recorded as slurry A;

[0040] (2) Weigh 838 g of calcined kaolin (solid content 98.5%), add 1257 g of water to make a slurry, add hydrochloric acid to adjust the pH value, and keep it for 30-90 min, which is recorded as slurry B;

[0041] (3) Slurries A and B were mixed evenly, 125 g of CaCl2 (CaO = 6%) was added, and the pH value was adjusted to 3.4-3.8, which was recorded as slurry C;

[0042] (4) Weigh 2000 g of alumina (ignition loss 35%) and add 3200 g of water, adjust the pH value to 1.8-2.5, and keep it for a period of time, which is recorded as slurry D;

[0043] (5) Weigh 6119 g of Y-type molecular sieve slurry (solid content 28.6%), add 1596.0 g of acetic acid (25 wt %) solution, and record it as slurry E;

[0044] (6) Slurries C, D, and E are added to a new reactor in sequence, mixed evenly, and then spray granulated, filtered, washed, and dried. The collected catalyst is recorded as Cat-2.

[0045] Comparative Example:

[0046] Weigh 683 g of kaolin (solid content 81.2%), add 721 g of water and 708 g of aluminum sol (Al2O3=21.2wt%), stir for more than 3 hours, continue to add 1780 g of Y-type molecular sieve (solid content 29.5%), 394 g of pseudo-boehmite (solid content 68.5%), and add a certain proportion of hydrochloric acid for acidification. After spray granulation, filtration, washing and drying, the obtained catalyst is recorded as DB-1.

[0047] Catalyst performance evaluation:

[0048] A FFB small fixed fluidized bed evaluation device was used.

[0049] The properties of the raw oil used for evaluation are as follows:

[0050] Table 1 Basic properties of crude oil

[0051]

[0052] The evaluation results are as follows:

[0053]

[0054] Judging from the evaluation data, gasoline, diesel and total liquid yields are significantly improved compared to the control agent, indicating that the catalyst prepared by this patent achieves the design goal. Of course, the present invention can also have many other embodiments, and technicians familiar with this field can make various corresponding deformations and adjustments based on the present invention, but these should all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a catalytic cracking catalyst with low coking and high gasoline and diesel production, comprising the following steps: (1) Add halloysite to a rotary granulation device, slowly add a certain proportion of an aqueous solution containing a first modifier while the device is rotating, stir thoroughly, introduce hot air to raise the temperature of the material to 60-85° C., maintain for 10-50 minutes, then transfer the material to a reactor, add water to slurry, filter and wash, add water to slurry again, add a second modifier, and the slurry is recorded as A for standby use; (2) calcined kaolin is slurried with water, and the third modifier is added to fully contact the slurry, which is recorded as B and set aside; (3) Slurry A and B are mixed, a certain proportion of the fourth modifier is added, and the pH value is adjusted to 3.4-3.

8. The slurry is recorded as C and is set aside; (4) Alumina is slurried with water to control the solid content and adjust the pH value to 1.8-2.5, and the slurry is kept for a period of time. The slurry is recorded as D and is set aside; (5) Add a certain proportion of acidic liquid to the Y-type molecular sieve for full contact. The slurry is recorded as E and is set aside. (6) Slurry C, slurry D and slurry E are added to a new reactor in sequence, mixed evenly, and then spray granulated, roasted, washed, filtered and dried to obtain a catalytic cracking catalyst with low coking and high gasoline and diesel production.

2. The preparation method according to claim 1, characterized in that: The first modifier is phosphoric acid, and the aqueous solution containing the first modifier is added in a ratio of (0.88-0.95)Pv·M, wherein Pv is the pore volume of halloysite, and M is the mass of halloysite. The concentration of the aqueous solution is 15-25wt% in terms of H3PO4.

3. The preparation method according to claim 1, characterized in that: In step (1), the second modifier is silica sol, and the added proportion is 3-8wt% of the final catalyst dry weight calculated as SiO2.

4. The preparation method according to claim 1, characterized in that: The third modifier in step (2) is hydrochloric acid.

5. The preparation method according to claim 1, characterized in that: The fourth modifier in step (3) is calcium chloride or magnesium chloride, and the added proportion is 0.05-0.18wt% of the final catalyst dry weight calculated as alkaline earth oxide.

6. The preparation method according to claim 1, characterized in that: The proportion of alumina added in step (4) is 18-26 wt% of the final catalyst dry weight in terms of Al2O3, and the alumina pore volume is 0.55-0.90 ml / g.

7. The preparation method according to claim 1, characterized in that: The Y-type molecular sieve described in step (5) is a unit cell constant The NaY is subjected to rare earth ion exchange and hydrothermal treatment, and the non-framework aluminum content is controlled to be ≤4.6wt%, and the addition ratio accounts for 30-40wt% of the final catalyst dry weight.

8. The preparation method according to claim 1, characterized in that: The acidic liquid in step (5) is formic acid or acetic acid, and the addition ratio is H + It is calculated as 0.0035-0.0045 of the Y-type molecular sieve dry basis.