Method for removing chlorinated pollutants in rectification residues
By treating the Joule heat of distilled residues and carbon black, the large energy consumption and secondary pollution problems of chlorine pollutants during chemical process are solved, efficient degradation and resource utilization are achieved, high-quality graphene nanosheets are generated, and high-quality graphene nanosheets are improved. Economic benefits of waste treatment.
Patent Information
- Application Number
- CN202410998130.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
When the prior art deals with chlorine pollutants in high-concentration distillation residues generated during chemical process, there are problems such as large energy consumption, cumbersome steps and secondary pollutants generation, making it difficult to achieve low-carbon and rapid harmless detoxification and Resource utilization.
By mixing the distilled residue with carbon black, the constant current power supply pulse discharge Joule heat treatment is carried out, and the current and resistance are controlled to quickly heat up, degrade chlorinated pollutants, and convert them into high-quality graphene nanosheets as a new wave absorbing material .
Achieve the degradation rate of more than 90% of chlorinated pollutants in the distilled residue, reduce energy consumption, avoid secondary pollution, and convert hazardous waste into high value-added graphene materials, improving the economic benefits of resource utilization .
Smart Images

Figure CN118926263A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of hazardous waste disposal, and in particular relates to a method for removing chlorinated pollutants in distillation residues. Background Art
[0002] With the rapid development of the chemical industry, more and more hazardous wastes are generated in the chemical process. Distillation residue refers to the substances that cannot be distilled out during the distillation process, mainly composed of high-boiling point or extremely unstable substances. The distillation residue produced in the joint production process of trichloroethylene and tetrachloroethylene contains high concentrations of new pollutants such as hexachlorobutadiene and other chlorinated pollutants (2000μg / g), which is much higher than the existing domestic control standards and regulations. It has been included in the national hazardous waste list control (HW11), waste code 261-018-11, hazardous characteristics T.
[0003] Due to the high concentration and complex organic matrix background, the room temperature wet advanced oxidation / reduction technology is not effective in treating chlorinated pollutants in distillation residues. The current disposal method for this type of distillation residue is co-incineration, which consumes a lot of energy and takes a long time to process. High concentrations of chlorinated pollution are difficult to completely degrade during incineration, and secondary pollutants such as dioxins are easily generated. Therefore, it is urgent to develop a low-carbon and fast method for harmless detoxification and resource utilization of distillation residues.
[0004] The invention patent application with publication number CN111635775A discloses a method for coking after blending phthalic anhydride distillation residue with coking blend coal, wherein by changing the mass ratio of the phthalic anhydride distillation residue and the coking blend coal, the resource utilization of the phthalic anhydride residue is achieved while ensuring the quality of coke. However, since the phthalic anhydride distillation residue contains phthalic anhydride, high molecular organic matter and organic carbonized matter, secondary pollution will be generated during high-temperature coking.
[0005] The invention patent application with publication number CN111187138A discloses a method in which glycerol and dichlorobenzene distillation residue are used as reaction raw materials and reacted under a hydrogen atmosphere to simultaneously produce reaction products including benzene, chlorobenzene and chloropropanol, thereby reducing the amount of three wastes generated. However, a large amount of additives are used, the technical solution steps are cumbersome, and the disposal cost and energy consumption are greatly increased.
[0006] The invention patent application with publication number CN111233621A discloses a hydrodechlorination reaction of dichlorobenzene distillation residue under the action of a precious metal catalyst in a fixed bed reactor. The precious metal catalyst greatly improves the conversion rate of polychlorobenzenes in the dichlorobenzene distillation residue and the selectivity of benzene, and has high industrial application value. However, a large amount of precious metal catalyst is used, which greatly increases the disposal cost.
[0007] From the above technical status and discussion, it can be seen that the current technologies for the disposal and resource utilization of distillation residues have many disadvantages such as complicated steps, generation of secondary pollutants, and high energy consumption of process routes. Therefore, it is urgent to explore a green, efficient and high-value technology for the disposal of high-concentration polluted distillation residues. Summary of the invention
[0008] The invention provides a method for removing chlorinated pollutants in distillation residues. The method can degrade chlorinated pollutants such as hexachlorobutadiene in the distillation residues of hazardous wastes.
[0009] The present invention provides a method for removing chlorinated pollutants in distillation residue, comprising:
[0010] S1, drying, grinding, sieving, and evenly mixing the distillation residue with carbon black to obtain a mixed powder;
[0011] S2. After extruding the mixed powder, Joule heat treatment is performed to remove chlorinated pollutants in the distillation residue. The Joule heat treatment is performed by pulse discharge of a constant current power supply. The discharge current is 10-80A and the discharge time is 1-10s.
[0012] Preferably, the mass percentage of the carbon black in the mixed powder is 5-20wt%. By providing sufficient carbon black, the electrical resistance of the mixed powder can be reduced to a suitable range while ensuring that the mixed powder can be conductive.
[0013] Preferably, the resistance of the extruded mixed powder is 5-20Ω. By controlling the resistance of the extruded mixed powder, the influence of the resistance on the thermal effect of the current is reduced as much as possible, and the Joule heat caused by the current is used to rapidly heat the extruded mixed powder.
[0014] Preferably, the carbon content of the distillation residue is 36-40 wt%, and graphene is obtained after removing chlorinated pollutants in the distillation residue.
[0015] Further preferably, the graphene is filled into a paraffin matrix to obtain an absorbing coating, the filling amount of the graphene in the absorbing coating is 30wt%, the thickness of the absorbing coating is 1.6mm, the absorbing performance is -42.037dB, and the effective absorption bandwidth is 3.94GHz.
[0016] The present invention successfully converts distillation residues into high-quality graphene nanosheets in a rapid Joule heating process, which can be used as a new type of absorbing material that meets the requirements of "thin, light, wide and strong", has higher benefits and application prospects, realizes high-value conversion of hazardous waste, and thus increases the economic benefits of hazardous waste treatment.
[0017] Preferably, before the constant current power supply pulse discharge, a pulse discharge is also performed, the discharge current of the pulse discharge is 30-60A, the discharge time is 1-2s, and there is a pause of 1-4s before the constant current power supply pulse discharge. By controlling the parameters of the first pulse discharge in advance, the resistance of the mixed powder is reduced to a suitable range, thereby more effectively increasing the Joule heat to improve the removal rate of chlorinated pollutants in the distillation residue.
[0018] Preferably, the chlorinated pollutant is one or more of hexachlorobutadiene, 1,1,3,3,4,4-hexachloro-1-butene, 1,1,2,3,3-pentachloropropane, pentachlorobenzene, hexachlorobenzene, and octachlorostyrene.
[0019] Preferably, the content of hexachlorobutadiene in the distillation residue is 1983.27 μg / g to 2449.96 μg / g.
[0020] Preferably, the distillation residue is the distillation residue produced by a vaporization tower in the joint production process of trichloroethylene and tetrachloroethylene.
[0021] Preferably, the mass percentage of each component element in the distillation residue is: carbon: 36-40wt%, hydrogen: 0.11-0.95wt%, nitrogen: 0.03-0.07wt%, sulfur: 0.25-0.62wt%, oxygen: 15-22wt%, chlorine: 28-34wt%, and inevitable impurities, and the sum of the mass percentages of carbon, hydrogen, nitrogen, sulfur, oxygen, chlorine and inevitable impurities is 100wt%.
[0022] Preferably, the distillation residue after screening is 40 mesh powder particles.
[0023] Preferably, based on the Joule heating effect of the current, after adjusting to the appropriate pulse discharge parameters, the heat release is determined, and in order to make the temperature reach the high temperature of 2800°C required for preparing graphene, the mass of the mixed powder needs to be limited. 0.1-0.2g of the mixed powder is taken for extrusion and Joule heating treatment.
[0024] Preferably, the step of extruding the mixed powder comprises:
[0025] The mixed powder is loaded into a quartz insulating tube, and conductive graphite plugs are installed at both ends to block the tube opening; the insulating quartz tube is installed on the sleeve fixing frame of the vacuum box, and the electrode rods at both ends are used to push the plugs along the axial direction, and the resistance of the mixed powder is measured at the same time. The density of the sample is adjusted by extrusion to control its resistance; the extrusion is stopped until the mixed powder is compacted and the resistance of the mixed powder reaches 5-20Ω.
[0026] Preferably, the power source used for the constant current power supply pulse discharge is a programmable direct current power source.
[0027] Preferably, the maximum temperature generated by the Joule heat is 400 to 3000°C.
[0028] Preferably, the yield of graphene after Joule heat treatment is 33-52%.
[0029] Preferably, after Joule heat treatment, pretreatments such as Soxhlet extraction, rotary evaporation, nitrogen blowing, constant volume, etc., qualitative and quantitative analysis and detection by GC-MS, the degradation rate of hexachlorobutadiene in the distillation residue can reach up to 99.08%.
[0030] Compared with the prior art, the beneficial effects of the present invention are:
[0031] The present invention controls the resistance of the mixed powder by extruding it, and controls the discharge current and discharge time to rapidly heat the mixed powder. Under the action of high temperature, the degradation rate of chlorinated pollutants in the distillation residue can reach more than 90%. Compared with traditional hazardous waste thermal disposal methods such as pyrolysis and incineration, the rapid Joule heat method provided by the present invention has lower energy consumption and no secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the Raman spectrum of the product obtained in Example 1 of the present invention;
[0033] Figure 2 This is a reflection loss curve diagram of the product obtained in Example 1 of the present invention;
[0034] Figure 3 This is the impedance matching diagram of the product obtained in Example 1 of the present invention;
[0035] Figure 4 This is a TEM image of the product obtained in Example 1 of the present invention;
[0036] Figure 5 This is a particle size distribution diagram of the product obtained in Example 1 of the present invention;
[0037] Figure 6 This is the Raman spectrum of the product obtained in Example 2 of the present invention;
[0038] Figure 7 This is the Raman spectrum of the product obtained in Example 3 of the present invention;
[0039] Figure 8 It is a comparison chart of the degradation rate-time of the hazardous waste containing hexachlorobutadiene treated in Examples 1 to 3 of the present invention and in Comparative Example 1;
[0040] Fig. 9 Gas chromatograms and removal efficiency diagrams of chlorinated pollutants in distillation residue and Joule thermal treatment products. DETAILED DESCRIPTION
[0041] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments:
[0042] In the experimental methods described in the following examples, unless otherwise specified, the power source adopts a 36V-83A programmable power source, and the discharge parameters are controlled by a PLC (programmable logic controller) control switch. The raw materials used are the distillation residues produced in the joint production process of trichloroethylene and tetrachloroethylene in a chemical plant in Zhejiang Province. The materials used can be obtained from commercial channels unless otherwise specified.
[0043] The present invention provides a method for rapidly degrading hexachlorobutadiene in hazardous waste by Joule heat and synthesizing graphene, wherein Joule heat is generated by pulse discharge of a constant current power supply, which is a resistance / ohm heating process, and the purpose of efficiently degrading high-concentration organic pollutant hexachlorobutadiene in hazardous waste residues is achieved by rapidly heating and cooling powder materials, and obtaining the high-quality graphene. The product can achieve ultra-high wave absorption performance of -42.037dB with an ultra-thin coating thickness of 1.6mm, and an effective absorption bandwidth of 3.94GHz, and has broad application potential and market prospects in the fields of stealth technology of aircraft, electromagnetic safety protection, and electromagnetic shielding of radar and communication equipment.
[0044] Pulse discharge uses a DC power supply to discharge multiple times in milliseconds to seconds, rapidly heats up and cools down, and achieves thermal shock to generate nano-scale material graphene. Pulse discharge can be used in two stages. By adjusting the discharge power and discharge time, different temperatures between 400 and 3000°C can be achieved. The temperature is mainly determined by the discharge voltage, the resistance of the reactants and the discharge current generated. Distillation residue is a poor conductor, so a small amount of conductive agent, i.e. carbon black, accounting for 20wt% of the sample is added to the raw powder of the distillation residue, and the sample resistance is controlled within a suitable range by electrode extrusion for Joule heating. Based on the current thermal effect, the Joule heat induced by the current can rapidly heat the sample. The degradation rate of organic pollutants in the distillation residue under high temperature can reach up to 99.08%. At the same time, high temperature and current can graphitize the sample into high-quality, high-value-added graphene, which can be used as a new type of absorbing material that meets the requirements of "thin, light, wide and strong". Realizing the high-value conversion of hazardous wastes has important scientific significance for the development of resource utilization technology of distillation residues.
[0045] Graphene is a carbon atom in the form of sp 2 The hybrid orbital is composed of a hexagonal honeycomb lattice of two-dimensional carbon nanomaterials, which has excellent optical, electrical, mechanical and thermal properties and is considered to be a revolutionary material in the future. The thickness of graphene is 0.335nm, which is only one layer of carbon atoms, but in fact, graphite structures with less than 10 layers can also be called graphene.
[0046] As a clear standard for detecting two-dimensional features, Raman spectroscopy has become the standard for judging graphene. For the Raman spectrum of graphene, its typical peaks appear at around 1350 wavenumbers, around 1580 wavenumbers, and around 2700 wavenumbers. Among them, the 1350 wavenumber peak is called the D peak, and its intensity corresponds to the degree of defects in graphene; the 1580 wavenumber peak is called the G peak, and its intensity corresponds to the degree of integrity of graphene. The wavenumber is called the 2D peak, which is a D peak overtone, and its intensity can represent the number of graphene layers. Generally speaking, the higher the 2D peak, the fewer the graphene layers, and the better the quality of the graphene. Commercial Graphene I 2D / I G ≈2, while the Raman spectrum of amorphous carbon does not have a 2D peak; according to the literature, I 2D / I G =0.10 as a benchmark. Specifically, for a single sampling point, 1) if I 2D / I G >0.10, the sample is graphene. 2) If I 2D / I G <0.10, the sample is not graphene. Based on these criteria, the Raman spectra of the products at different pulse times provided in Examples 1-3 of the present invention indicate that the hazardous waste distillation residues are successfully converted into high-quality graphene.
[0047] Example 1
[0048] Add 0.2g of carbon black powder to 1.0g of 40-mesh distillation residue powder that has been ground and sieved, mix and stir evenly to obtain 1.2g of residue and carbon black mixture powder. Take 0.15g of the above mixture powder and put it into a quartz tube with an inner diameter of 8mm, plug both ends of the quartz tube with a diameter of 8mm, and put it into the reaction box sleeve fixing frame. Rotate the electrode rod knob to move the graphite plug along the axis, gently compress the mixed powder and measure the resistance at both ends until the material is compressed and difficult to compress and the resistance is in the appropriate range (5.0~20.0Ω), then stop compressing. Install the temperature probe, close the vacuum box, and evacuate the box to reduce the air pressure to 0.02MPa to prevent internal explosion.
[0049] Turn on the DC power supply, set the pulse discharge voltage to 30V, the first stage discharge current to 40A, set the discharge time to 1s, pause for 3s, the second stage discharge current to 80A, set the discharge time to 10s. Perform pulse discharge and monitor the temperature in the quartz tube. During discharge, the mixture powder emits a dazzling white light, the maximum current is 80A, and the highest temperature reaches 3000℃. After the discharge is completed, cool to room temperature, take out the quartz tube, pour out the slightly gray mixture powder after the reaction, weigh and calculate the reaction mass yield.
[0050] The raw material hazardous waste residue and the product of the pulse Joule heat of this embodiment were respectively analyzed and tested for hexachlorobutadiene. After GC-MS analysis and testing, combined with the mass yield after the reaction, the degradation rate of hexachlorobutadiene was 99.08%.
[0051] The product after pulse Joule heating in this embodiment is taken for laser Raman spectroscopy detection. Figure 1 The treated sample has a strong 2D peak. The intensity of the 2D band relative to the G band (I 2D / I G ) is greater than 2. The extremely low intensity of the D band indicates a low defect concentration in the pulsed Joule heating product, which contributes to the amplification of the 2D band, which may be the result of the extreme temperature reached during the pulsed Joule heating process, which drives non-carbon elements out of the system. Graphitization occurs in organic compounds after high-temperature annealing. During graphitization, organic materials are heated to increase the carbon content through pyrolysis. During pyrolysis, carbon forms sp 2 Hybridized covalent bonds and crystallized into layered graphite domains. Therefore, Raman spectroscopy showed that the rapid Joule heating method achieved the generation of high-quality graphene materials.
[0052] The graphene produced in this embodiment was mixed with paraffin, and when the mass fraction of the graphene was 30%, its wave absorbing performance was tested by a vector network analyzer (Keysight, N5234B), and the test frequency was 2-18 GHz. Figure 2 It can be seen that at 14.58 GHz, the minimum reflection loss value reaches -42.037 dB, the effective absorption bandwidth is 3.94 GHz, and the matching thickness is only 1.6 mm.
[0053] Figure 3 This is the impedance matching diagram of the graphene product of this embodiment. It can be seen that under the thickness of the absorbing coating, in the frequency range of 2 GHz-18 GHz, the impedance matching |Z| value is close to 1 (the specific variation range is 0.998-1.176).
[0054] The product of the 10s pulse was taken for TEM characterization. Figure 4 The size and morphology of the graphene product can be seen. The average size of the graphene flakes is 38.56±9.90nm. Figure 5 It is the particle size distribution characteristic of graphene product.
[0055] The product of the 10s pulse was tested for its wave absorption performance using a vector network analyzer (Keysight, N5234B) at a test frequency of 2-18 GHz. Figure 2 It can be seen that at 14.58 GHz, the minimum reflection loss value reaches -42.037 dB, the effective absorption bandwidth is 3.94 GHz, and the matching thickness is only 1.6 mm.
[0056] To achieve efficient electromagnetic wave absorption, the electromagnetic waves must first be able to enter the absorbing material to the greatest extent possible, rather than being reflected back into the air from the surface of the material. Therefore, this requires that the absorbing material has good electromagnetic parameters and good impedance matching characteristics. The closer |Z| is to 1, the more electromagnetic waves enter the material. Figure 3 This is the impedance matching diagram of the graphene product. It can be seen that under the thickness of the absorbing coating, in the frequency range of 2GHz-18GHz, the impedance matching |Z| value is close to 1 (the specific variation range is 0.998–1.176).
[0057] Example 2
[0058] In this embodiment, the sample selection is the same as that in Embodiment 1.
[0059] The operation process of this embodiment is consistent with that of embodiment 1, and some parameters in each step are adjusted as follows:
[0060] Add 0.2g of carbon black powder to 1.0g of 40-mesh distillation residue powder that has been ground and sieved, mix and stir evenly to obtain 1.2g of residue and carbon black mixture powder. Take 0.15g of the above mixture powder and put it into a quartz tube with an inner diameter of 8mm, plug both ends of the quartz tube with a diameter of 8mm, and put it into the reaction box sleeve fixing frame. Rotate the electrode rod knob to move the graphite plug along the axis, gently compress the mixed powder and measure the resistance at both ends until the material is compressed and difficult to compress and the resistance is in the appropriate range (5.0~20.0Ω), then stop compressing. Install the temperature probe, close the vacuum box, and evacuate the box to reduce the air pressure to 0.02MPa to prevent internal explosion.
[0061] Turn on the DC power supply, set the pulse discharge voltage to 30V, the first stage discharge current to 40A, the discharge time to 1s, the interval to 3s, the second stage discharge current to 80A, the discharge time to 7.5s. Perform pulse discharge and monitor the temperature in the quartz tube. During discharge, the mixture powder emits a dazzling white light, the maximum current is 80A, and the highest temperature reaches 2650℃. After the discharge is completed, cool to room temperature, take out the quartz tube, pour out the slightly gray mixture powder after the reaction, weigh and calculate the reaction mass yield.
[0062] The raw material hazardous waste residue and the product of pulse Joule heat were respectively analyzed and tested for hexachlorobutadiene. After GC-MS analysis and detection, combined with the mass yield after the reaction, the degradation rate of hexachlorobutadiene was 93.34%.
[0063] The product after pulse Joule heating is detected by laser Raman spectroscopy. Figure 6 The treated sample has a strong 2D peak. The intensity of the 2D band relative to the G band (I 2D / I G) is 1.3. Raman spectroscopy shows that the rapid Joule heating method achieves the generation of high-quality graphene materials.
[0064] Example 3
[0065] In this embodiment, the sample selection is the same as that in Embodiment 1.
[0066] The operation process of this embodiment is consistent with that of embodiment 1, and some parameters in each step are adjusted as follows:
[0067] Add 0.2g of carbon black powder to 1.0g of 40-mesh distillation residue powder that has been ground and sieved, mix and stir evenly to obtain 1.2g of residue and carbon black mixture powder. Take 0.15g of the above mixture powder and put it into a quartz tube with an inner diameter of 8mm, plug both ends of the quartz tube with a diameter of 8mm, and put it into the reaction box sleeve fixing frame. Rotate the electrode rod knob to move the graphite plug along the axis, gently compress the mixed powder and measure the resistance at both ends until the material is compressed and difficult to compress and the resistance is in the appropriate range (5.0~20.0Ω), then stop compressing. Install the temperature probe, close the vacuum box, and evacuate the box to reduce the air pressure to 0.02MPa to prevent internal explosion.
[0068] Turn on the DC power supply, set the pulse discharge voltage to 30V, the first stage discharge current to 40A, set the discharge time to 1s, pause for 3s, the second stage discharge current to 80A, set the discharge time to 5s. Perform pulse discharge and monitor the temperature in the quartz tube. During discharge, the mixture powder emits a dazzling white light, the maximum current is 80A, and the highest temperature reaches 2600℃. After the discharge is completed, cool to room temperature, take out the quartz tube, pour out the slightly gray mixture powder after the reaction, weigh and calculate the reaction mass yield.
[0069] The raw material hazardous waste residue and the product of pulse Joule heat were respectively analyzed and tested for hexachlorobutadiene. After GC-MS analysis and detection, combined with the mass yield after the reaction, the degradation rate of hexachlorobutadiene was 91.17%.
[0070] The product after pulse Joule heating is detected by laser Raman spectroscopy. Figure 7 The treated sample has a strong 2D peak. The intensity of the 2D band relative to the G band (I 2D / I G ) is 0.80. Raman spectroscopy shows that the rapid Joule heating method achieves the generation of high-quality graphene materials.
[0071] Comparative Example 1
[0072] Different from Example 1, the distillation residue powder is directly pyrolyzed at a temperature of 500° C. and a pyrolysis time of 40 min.
[0073] like Figure 8 As shown, the Joule heat treatment method provided in Examples 1-3 of the present invention has a higher degradation rate for removing hexachlorobutadiene hazardous waste than the pyrolysis method in the prior art, and the degradation time is extremely short.
[0074] like Fig. 9 As shown, the degradation effect on other chlorinated pollutants is also significant. After 10 seconds of pulse, the degradation rates of 1,1,3,3,4,4-hexachloro-1-butene, 1,1,2,3,3-pentachloropropane, pentachlorobenzene, hexachlorobenzene and octachlorostyrene are 92.56%, 98.64%, 99.83%, 99.23% and 99.97%, respectively.
[0075] Finally, it should be noted that the above examples are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above examples, and many variations are possible. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A method for removing chlorinated pollutants from distillation residues, characterized in that: include: S1, drying, grinding, sieving, and evenly mixing the distillation residue with carbon black to obtain a mixed powder; S2. After extruding the mixed powder, Joule heat treatment is performed to remove chlorinated pollutants in the distillation residue. The Joule heat treatment is performed by pulse discharge of a constant current power supply. The discharge current is 10-80A and the discharge time is 1-10s.
2. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: The mass percentage of carbon black in the mixed powder is 5 to 20 wt%.
3. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: The electrical resistance of the extruded mixed powder is 5-20Ω.
4. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: The carbon content of the distillation residue is 36-40wt%, and graphene is obtained after removing chlorinated pollutants in the distillation residue.
5. The method for removing chlorinated pollutants in distillation residue according to claim 4, characterized in that: The graphene is filled into a paraffin matrix to obtain a wave-absorbing coating, in which the filling amount of the graphene in the wave-absorbing coating is 30wt%, the thickness of the wave-absorbing coating is 1.6mm, the wave-absorbing performance is -42.037dB, and the effective absorption bandwidth is 3.94GHz.
6. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: Before the constant current power supply pulse discharge is performed, another pulse discharge is performed. The discharge current of the pulse discharge is 30-60A, the discharge time is 1-2s, and there is a pause of 1-4s before the constant current power supply pulse discharge is performed.
7. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: The distillation residue is a chlorinated hydrocarbon distillation residue, which is produced in the joint production process of trichloroethylene and tetrachloroethylene and contains high-concentration chlorinated pollutants. The high-concentration chlorinated pollutants are one or more of hexachlorobutadiene, 1,1,3,3,4,4-hexachloro-1-butene, 1,1,2,3,3-pentachloropropane, pentachlorobenzene, hexachlorobenzene, and octachlorostyrene.
8. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: The mass percentages of the component elements in the distillation residue are: carbon: 36-40wt%, hydrogen: 0.11-0.95wt%, nitrogen: 0.03-0.07wt%, sulfur: 0.25-0.62wt%, oxygen: 15-22wt%, chlorine: 28-34wt%, and inevitable impurities, and the sum of the mass percentages of carbon, hydrogen, nitrogen, sulfur, oxygen, chlorine and inevitable impurities is 100wt%.
9. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: The step of extruding the mixed powder comprises: The mixed powder is loaded into a quartz insulating tube, and conductive graphite plugs are installed at both ends to block the tube opening; the insulating quartz tube is installed on the sleeve fixing frame of the vacuum box, and the electrode rods at both ends are used to push the plugs along the axial direction, and the resistance of the mixed powder is measured at the same time. The density of the sample is adjusted by extrusion to control its resistance; the extrusion is stopped until the mixed powder is compacted and the resistance of the mixed powder reaches 5-20Ω.
10. The method for removing chlorinated pollutants in distillation residue according to claim 1, characterized in that: The temperature generated by the Joule heat treatment is 400 to 3000°C.
Citation Information
Patent Citations
Method for preparing graphene oxide / white carbon black / rubber nanocomposite
CN102604175A
Positive electrode active material, positive electrode containing positive electrode active material, and lithium secondary battery
CN109817907A
Double-layer polymer-based electric response shape memory material and preparation method thereof
CN111516338A
Plasma high-temperature melting carbonaceous mixed solid waste treatment system and treatment method
CN115662673A
Method for preparing graphene oxide from waste organic matters
CN118145632A