Worm grinding wheel, method for manufacturing worm grinding wheel and application of worm grinding wheel

By using the single-piece structure of the transition section in the worm grinding wheel, the abrasive particles of different particle characteristics are embedded in the same matrix material, the problem of weak positions connecting the existing worm grinding wheel is solved, and low-cost and robust grinding is achieved and trimming effect.

CN118926625APending Publication Date: 2024-11-12KLINGELNBERG AG
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410572474.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing worm grinding wheels have defects in connecting weak positions during manufacturing and use, resulting in unstable and costly during grinding and trimming.

Method used

Design a worm grinding wheel, whose two areas with different particle characteristics form transition sections through original molding to form a single-piece structure, avoiding joint and bonding positions, and embed coarse and fine abrasive particles in it with the same matrix material to ensure the material Locking connection.

Benefits of technology

The low-cost manufacturing of worm grinding wheels and the robustness during grinding and dressing are achieved, and the defects of weak connections are avoided and the service life is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926625A_ABST
    Figure CN118926625A_ABST
Patent Text Reader

Abstract

The invention relates to a worm grinding wheel, the worm grinding wheel being a dressable worm grinding wheel, a first section of the worm grinding wheel having first abrasive grains incorporated in a matrix material, a second section of the worm grinding wheel having second abrasive grains incorporated in the matrix material, the first abrasive particles and the second abrasive particles differ from each other in terms of particle size and / or particle material, a transition section is formed between the first section and the second section, both the first abrasive particles and the second abrasive particles are incorporated into the matrix material, and wherein the first abrasive particles and the second abrasive particles are incorporated into the matrix material. The first section, the second section and the transition section have the same matrix material, and wherein in the transition section, a blending of the first abrasive grains and the second abrasive grains is formed at least in sections.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a grinding worm and a method for producing the grinding worm and the use of the grinding worm. Background Art

[0002] Grinding worms are used for grinding gears in the continuous grinding method of rolling grinding. Typical examples of gears that can be finished by rolling grinding are, for example, spur gears or helical gears.

[0003] Roller grinding itself can be carried out in several steps, wherein first a greater material removal is carried out in a first overrun, the so-called roughing or rough grinding, wherein subsequently a smaller material removal is carried out in one or more further overruns, the so-called finishing or finishing grinding. Depending on the required quality, a distinction can be made between finishing grinding and polishing grinding in terms of finishing.

[0004] It can be seen that for rough grinding, coarser abrasive grains can be used than for fine grinding. In order not to have to provide a dedicated grinding worm with the correspondingly required abrasive grains for each working step, it is known to use grinding worms with both coarse and fine abrasive grains. For example, these grinding worms are provided so that a first module of the relevant grinding worm has coarse abrasive grains with a ceramic bond and a second module of the grinding worm has fine abrasive grains with a resin bond. The two modules are, for example, bonded to one another in order to provide a grinding worm with two different grain compositions in this way. However, each of the two modules is first manufactured separately and independently of the other module. In other words, this involves two separate grinding worms of different grain compositions, which are assembled to form one grinding worm.

[0005] Such grinding worms are therefore complex in terms of their production, wherein the connection point between the two modules represents a weak point which can lead to defects at the connection point during use of the respective grinding worm or during dressing. Summary of the invention

[0006] Against this background, the invention is based on the technical problem of providing an improved grinding worm having at least two grain compositions or at least two regions with different removal properties, which is particularly cost-effective to produce and is also robust over its entire service life, and more precisely both during grinding and during dressing. Furthermore, a method for producing and using such a grinding worm is to be provided.

[0007] The above technical problems are solved by the independent claims, respectively. Further embodiments of the present invention are obtained from the dependent claims and the following description.

[0008] According to a first aspect, the invention relates to a grinding worm, wherein the grinding worm is a dressable grinding worm, wherein a first section of the grinding worm has first abrasive particles incorporated into a matrix material, wherein a second section of the grinding worm has second abrasive particles incorporated into the matrix material, wherein the first abrasive particles and the second abrasive particles differ from one another in terms of particle size and / or particle material and / or shape, wherein a transition section is formed between the first section and the second section, in which transition section both the first abrasive particles and the second abrasive particles are incorporated into the matrix material, wherein the first section, the second section and the transition section have the same matrix material, and wherein in the transition section a mixture of the first abrasive particles and the second abrasive particles is formed at least in sections.

[0009] The first section and the second section are connected to each other in particular by initial shaping, so that the transition section forms a material-locking connection of the first section to the second section. In other words, the first section, the second section and the transition section are provided integrally as a one-piece blank by initial shaping, so that no joining points and no bonding points are formed between the first section and the second section.

[0010] The grinding worm configured in the manner according to the invention can therefore be manufactured particularly cost-effectively and also robustly over its entire service life, and more precisely both during grinding and during dressing. This can be achieved in particular by embedding both the first abrasive grain and the second abrasive grain in the same matrix material in a preformed manner.

[0011] If the particle size of the abrasive grains is mentioned here, this refers in particular to the average particle size, wherein the average particle size can be defined in particular by a particle size range. For example, it can be provided that the average particle size of the first abrasive grains is in the range of 0.06 mm to 0.12 mm, while the average particle size of the second abrasive grains is in the range of 0.14 mm to 0.22 mm. In this case, the second abrasive grains are therefore coarser abrasive grains, while the first abrasive grains are finer abrasive grains relative thereto.

[0012] Depending on the design of the grinding worm, it is provided that the first section has coarser abrasive grain than the second section, or vice versa.

[0013] The first abrasive grains may be a mixture of abrasive grains. The second abrasive grains may be a mixture of abrasive grains.

[0014] The first abrasive grains may be made of corundum or aluminum oxide.

[0015] The first abrasive grains may be composed of silicon carbide.

[0016] The first abrasive grains may be composed of cubic boron nitride. The first abrasive grains may be composed of synthetic diamond.

[0017] The first abrasive grains may have a mixture of abrasive grains composed of two or more materials among the above-mentioned materials.

[0018] The second abrasive grains may be made of corundum or aluminum oxide.

[0019] The second abrasive grains may be made of silicon carbide. The second abrasive grains may be made of cubic boron nitride.

[0020] The second abrasive grain may be composed of synthetic diamond.

[0021] The second abrasive grains may have a mixture of abrasive grains composed of two or more materials among the above-mentioned materials.

[0022] It can be provided that the grinding worm is a ceramic bonded grinding worm. Accordingly, the matrix material is a ceramic bond.

[0023] The matrix material may include one or more of the following materials: clay, kaolin, feldspar, quartz and porcelain powder, calcite, iron oxide, glass frit. The matrix material may be, for example, an amorphous bond, i.e. a melt bond with a high glass phase content, or, for example, a bond with a medium glass phase content, or, for example, a porcelain-like sintered bond, i.e. a sintered bond with a small glass phase content or no glass phase content.

[0024] According to an alternative embodiment, it can be provided that the grinding worm has a resin bond as a matrix material.

[0025] The first abrasive particles and / or the second abrasive particles can differ from one another in terms of their shape, wherein the first abrasive particles and the second abrasive particles can in particular each have different shapes or configurations selected from the group consisting of: hexahedron, rhombohedron, tetrahedron, octahedron, pyramid, trapezoidal hedron, prism.

[0026] The first section and the second section can differ from each other with respect to their porosity. Thus, the first section can have a greater porosity than the second section, or vice versa.

[0027] The first section and the second section can differ from each other with regard to their pore size. Thus, the first section can have a larger pore than the second section, or vice versa.

[0028] In particular, the grinding worm is not a galvanically coated grinding worm.

[0029] It can be provided that the first section has a first modified contour shape and the second section has a second modified contour shape, wherein the geometry of the modified first contour shape differs from the geometry of the modified second contour shape, wherein the grinding worm is provided for topological grinding of a toothing.

[0030] The term "topological grinding" according to the invention includes not only classic variants for producing toothing, such as setbacks in the area of ​​the tooth tip, tooth root or tooth end, convexities in the contour direction and / or tooth flank direction or angular variants in the contour direction and / or tooth flank direction, but also superpositions of classic variants. Furthermore, the term "topological grinding" according to the invention includes variants for producing toothing, in which the tooth flank of the toothing is regarded as a grid or free-form surface and the change values ​​are freely preset with the aid of sampling points on this grid. Thus, any modified tooth flank shape can be defined, which is not restricted to a preset catalog of predefined toothing variants. In this context, the term "any modified tooth flank shape" is restricted to tooth flank shapes that enable an operational toothing.

[0031] According to a second aspect, the present invention relates to a method having the following method steps: providing first abrasive particles; providing second abrasive particles; providing a matrix material; mixing the first abrasive particles with the matrix material to form a first mixture; mixing the second abrasive particles with the matrix material to form a second mixture; stacking the first mixture and the second mixture in layers in a mold; pressing the first mixture and the second mixture in the mold and sintering the first and second mixtures into a cylindrical blank; producing a grinding worm by profiling the blank; wherein the grinding worm is constructed according to the present invention.

[0032] After pressing, a green body is produced, which can first be dried and then fired or sintered by heat input to form a green body. The matrix material can contain volatile materials or pore formers which degas or burn or oxidize during combustion.

[0033] According to a third aspect, the invention relates to a method having the following method steps: providing a grinding worm according to the invention; providing a component having a toothing to be ground; grinding the tooth flanks of the toothing by means of a first section; grinding the tooth flanks of the toothing by means of a second section.

[0034] It can be provided that a first section of the grinding wheel worm has a first dressed contour shape and a second section of the grinding wheel worm has a second dressed contour shape, wherein the geometry of the dressed first contour shape is different from the geometry of the dressed second contour shape, wherein the grinding wheel worm is configured for topological grinding of a tooth portion, and the grinding of the tooth flanks of the tooth portion is topological grinding. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The invention is explained in more detail below with the aid of the accompanying drawings showing exemplary embodiments. They are schematically shown:

[0036] Figure 1 Shows a worm grinding wheel according to the present invention;

[0037] Figure 2 A mold for sintering is shown;

[0038] Figure 3A A cylindrical green body is shown;

[0039] Figure 3B A cylindrical, uncontoured blank is shown;

[0040] Figure 4 Shows the basis for the contouring of the blank Figure 1 Worm grinding wheel;

[0041] Figure 5 A flow chart showing a grinding method according to the present invention;

[0042] Fig. 6A Grinding is shown using a first section of a worm grinding wheel;

[0043] Figure 6B Grinding with the second section of the grinding worm is shown. DETAILED DESCRIPTION

[0044] Figure 1 A grinding worm 10 according to the invention is shown in a side view.

[0045] The grinding worm 10 is a dressable grinding worm. The grinding worm 10 has an axis of rotation R, about which the grinding worm 10 is rotationally driven or rotated during operation.

[0046] The first section 12 of the grinding worm 10 has first abrasive grains 14 . The first abrasive grains 14 are integrated into a matrix material 16 .

[0047] Second section 18 of grinding wheel worm 10 has second abrasive grains 20 which are also integrated into matrix material 16 .

[0048] The first abrasive grains 14 and the second abrasive grains 20 are different from each other in their grain sizes. Here, the second abrasive grains 20 have an average grain size that is smaller than the average grain size of the first abrasive grains 14 .

[0049] A transition section 22 is formed between the first section 12 and the second section 18 . In the transition section 22 , both the first abrasive grains 14 and the second abrasive grains 20 are incorporated into the matrix material 16 .

[0050] The first section 12 , the second section 18 and the transition section 22 comprise the same matrix material 16 . In the transition section 22 , a mixture of the first abrasive grains 14 and the second abrasive grains 20 is formed.

[0051] The first section 12 extends along a length L1 as viewed with respect to the rotation axis R. The transition section 22 extends along a length L2 as viewed with respect to the rotation axis R. The second section 18 extends along a length L3 as viewed with respect to the rotation axis R.

[0052] In the region of first section 12 , grinding wheel worm 10 therefore has first abrasive grains 14 and in particular no second abrasive grains 20 . In the region of second section 18 , grinding wheel worm 10 therefore has second abrasive grains 20 and in particular no first abrasive grains 14 .

[0053] It should be understood that during the manufacture of the grinding worm 10, it may happen that some of the first abrasive particles 14 enter the second section 18, and conversely, some of the second abrasive particles 20 enter the region of the first section 12. However, the first section 12 mainly has the first abrasive particles 14, that is, for example, more than 90% or more than 95% of the first abrasive particles, in particular more than 98% of the first abrasive particles. Correspondingly, the second section 18 mainly has the second abrasive particles 20, that is, for example, more than 90% or more than 95% of the second abrasive particles 20, in particular more than 98% of the second abrasive particles.

[0054] The above percentage values ​​relate only to the abrasive grain content of the relevant first section 12 and the relevant second section 18, but not to the total material volume of the relevant sections 12, 18. This is because the grinding worm 10 as a whole consists of abrasive grains 14, 20, holes 24 and base material 16. Figure 1 , which is intended to illustrate in a greatly simplified manner the composition and material distribution of grinding worm 10 in the individual regions 12 , 18 , 22 .

[0055] Grinding worm 10 is a vitrified bonded grinding worm in this case.

[0056] Refer to the following Figure 2 , 3A , 3B and 4 describe the manufacture of the grinding worm 10 according to the present invention.

[0057] First, the first abrasive particles 14 and the second abrasive particles 20 are provided.

[0058] The first abrasive particles 14 and the second abrasive particles 20 are each mixed individually and independently of each other with the matrix material 16. In this way, the first abrasive particles 14 are mixed with the matrix material 16 to give a first mixture M1, and the second abrasive particles 20 are mixed with the matrix material 16 to give a second mixture M2.

[0059] The first mixture M1 is then first introduced into the mold 26 and the second mixture M2 is then introduced into the same mold 26. The first mixture M1 and the second mixture M2 are thus stacked in layers within the mold 26 and then pressed into a cylindrical green body G by pressure application P.

[0060] Therefore, the result of suppression is Figure 3A The cylindrical green compact G shown in FIG. 1 already comprises a first section 12 with a corresponding abrasive grain distribution, a second section 18 and a transition section 22. Then, by introducing heat W, the green compact G is sintered into a cylindrical blank 28.

[0061] The result of sintering is Figure 3B The cylindrical blank 28 shown in FIG. 1 already comprises a first section 12, a second section 18 and a transition section 22 with a corresponding abrasive grain distribution. Finally, the grinding worm 10 is manufactured by contouring the blank 28 with the aid of a tool 30 ( Figure 4 ), wherein the tool 30 can be a trimmer, for example.

[0062] Figure 5 A flow chart of the grinding method according to the invention is schematically shown.

[0063] In a first method step (A), a grinding worm 10 is provided.

[0064] In a second method step (B), a component 32 having a toothing 34 to be ground is provided.

[0065] In a third method step (C), the tooth flanks 36 of the toothing 34 are ground by means of the first section 12 of the grinding tool 10 ( Fig. 6A ).

[0066] In a fourth method step (D), the tooth flanks 36 of the toothing 34 are ground by means of the second section 18 of the grinding tool 10 ( Figure 6B ).

[0067] In this example, the first section 12 has a modified first contour shape 38. In this example, the second section 18 has a modified second contour shape 40, wherein the geometry of the modified first contour shape 38 is different from the geometry of the modified second contour shape 40,

[0068] The grinding worm 10 is provided for topological grinding of the toothing 34 , and the grinding of the tooth flanks 36 of the toothing 34 is topological grinding.

[0069] The segment 12 can be configured for roughing. The segment 18 can be configured for finishing. The grinding worm 10 can have a plurality of segments 18 for finishing, which each have a different contour shape for topological grinding.

[0070] Reference numerals list

[0071] 10 Worm Grinding Wheel

[0072] 12 First Segment

[0073] 14 First abrasive grain

[0074] 16 Base material

[0075] 18 Second Section

[0076] 20 Second abrasive grain

[0077] 22 Transition section

[0078] 24 holes

[0079] 26 Mould

[0080] 28 Blanks

[0081] 30 Tools

[0082] 32 Components

[0083] 34 teeth

[0084] 36 tooth surface

[0085] 38 Outline Shape

[0086] 40 Outline Shapes

[0087] (A) Methods and Steps

[0088] (B) Methods and Steps

[0089] (C) Methods and Steps

[0090] (D) Methods and Steps

[0091] L1 Length

[0092] L2 Length

[0093] L3 Length

[0094] R blank

[0095] P Pressure

[0096] W Heat

Claims

1. A worm grinding wheel, - wherein the worm grinding wheel (10) is a dressable worm grinding wheel, -in, The first section (12) of the grinding worm (10) has first abrasive grains (14) incorporated in a matrix material (16). wherein the second section (18) of the grinding worm (10) has second abrasive grains (20) incorporated into the matrix material (16), wherein the first abrasive grain (14) and the second abrasive grain (20) differ from one another in terms of grain size and / or grain material and / or shape, wherein a transition section (22) is formed between the first section (12) and the second section (18), in which both the first abrasive grains (14) and the second abrasive grains (20) are incorporated into the matrix material (16), - wherein the first section (12), the second section (18) and the transition section (22) have the same base material (16), and - wherein in the transition section (22), a mixing of the first abrasive grain (14) and the second abrasive grain (20) is at least partially formed.

2. The worm grinding wheel according to claim 1, characterized in that: - the first section (12) and the second section (18) are connected to each other by initial forming, wherein the transition section (22) forms a material-locking connection between the first section (12) and the second section (18).

3. A grinding worm according to any one of the preceding claims, characterized in that - the first section (12) has a coarser abrasive grain than the second section (18), or The second section (18) has a coarser abrasive grain than the first section (12).

4. A grinding worm according to any one of the preceding claims, It is characterized in that - the first abrasive particles are a mixture of abrasive particles, and / or The second abrasive particles can be a mixture of abrasive particles.

5. A grinding worm according to any one of the preceding claims, characterized in that - the first abrasive grains consist of corundum, or - the first abrasive grains consist of silicon carbide, or - the first abrasive grains are composed of cubic boron nitride, or - the first abrasive grains consist of synthetic diamond, or The first abrasive grains are composed of a mixture of abrasive grains composed of two or more materials selected from the group consisting of corundum, silicon carbide, cubic boron nitride, and synthetic diamond.

6. A grinding worm according to any one of the preceding claims, characterized in that - the second abrasive grains consist of corundum, or - the second abrasive grains consist of silicon carbide, or - the second abrasive grains consist of cubic boron nitride, or - the second abrasive grains consist of synthetic diamond, or The second abrasive grains are composed of a mixture of abrasive grains composed of two or more materials selected from the group consisting of corundum, silicon carbide, cubic boron nitride, and synthetic diamond.

7. A grinding worm according to any one of the preceding claims, characterised in that The worm grinding wheel (10) is a ceramic-bonded worm grinding wheel (10).

8. A grinding worm according to any one of the preceding claims, characterised in that The matrix material comprises one or more of the following materials: clay, kaolin, feldspar, quartz and porcelain powder, calcite, iron oxide, and glass frit.

9. A grinding worm according to any one of the preceding claims, characterised in that The worm grinding wheel is not a worm grinding wheel with an electroplating coating.

10. A grinding worm according to any one of the preceding claims, characterised in that - the first section has a modified first contour shape (38), and - the second section has a modified second contour shape (40), - wherein the geometry of the modified first contour shape (38) is different from the geometry of the modified second contour shape (40), - wherein the grinding worm (10) is configured for topological grinding of the toothing (34).

11. A method comprising the following steps: - providing first abrasive particles (14); - providing second abrasive particles (20); - providing a matrix material (16); - mixing the first abrasive particles (14) with the matrix material (16) into a first mixture (M1); - mixing the second abrasive particles (20) with the matrix material (16) into a second mixture (M2); - stacking the first mixture (M1) and the second mixture (M2) in layers in a mold (26), - pressing the first mixture (M1) and the second mixture (M2) in the mold (26) and sintering the first and second mixtures into a cylindrical blank (28); - manufacturing a grinding worm (10) by profiling the blank (28); -in, The grinding worm (10) is configured according to any one of claims 1 to 10.

12. A method comprising the following steps: - Providing a grinding worm (10) according to any one of claims 1 to 10; - providing a component (32) having a toothing (34) to be ground; - grinding the tooth flanks (36) of the toothing (34) by means of the first section (12); - grinding the tooth flanks (36) of the toothing (34) by means of the second section (18).

13. The method according to claim 12, characterized in that - the grinding worm is constructed according to claim 10, and The grinding of the tooth flanks (36) of the toothing (34) is topological grinding.

Citation Information

Cited By

  • Double-layer worm grinding wheel for high-precision gear grinding and preparation method of double-layer worm grinding wheel