Preparation and hot pressing method of self-crosslinking adhesive with high lignin content
The ultra-high lignin adhesive prepared by hydrothermal assisted synthesis method solves the problems of toxic substance release and insufficient performance in plywood adhesives, and realizes the production of high-performance plywood, which has good thermal stability and easy to produce on a large scale.
Patent Information
- Application Number
- CN202411038252.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
Smart Images

Figure BSA0000299630740000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wood processing and manufacturing, and relates to a method for preparing plywood by cross-linking and hot pressing using lignin as an adhesive raw material. Background Art
[0002] Plywood is widely used in construction, such as floors and interior walls, as well as in the manufacture of household items such as furniture and cabinets. With the increasing awareness of forest resource protection, people are increasingly using artificial board furniture instead of solid wood furniture, which has led to an increasing use of adhesives. As a key raw material for plywood, adhesives directly determine the strength, water resistance, heat resistance, etc. of plywood and the cost of plywood. In addition, the current adhesives for artificial boards are mainly "trialdehyde glue", which mainly uses formaldehyde, urea, melamine, phenol, etc. as raw materials. During the production, transportation and use, toxic and harmful substances such as formaldehyde and phenol will be released, which will cause irreversible harm to human health and also affect the sustainable development of society. Therefore, it has become a trend to adopt new environmentally friendly processes and find green raw materials to develop high-performance adhesives.
[0003] Lignin is present in the cell walls of almost all terrestrial plants and is the most abundant aromatic biopolymer on earth. In lignocellulose, lignin acts as a binder, providing strength to the cell wall by effectively binding cellulose and hemicellulose together. Structurally, lignin is formed by the oxidative coupling of plant phenolic monomers. The randomness of the connections between various types of monomers, the presence of modifiable functional group sites (methoxy, alcohol hydroxyl, phenolic hydroxyl, carbonyl, etc.), and the complex three-dimensional structure give lignin a variety of natural properties (adhesion, hydrophobicity, antioxidant, UV shielding, etc.), and make lignin have great potential for modification and functionalization.
[0004] The purpose of the present invention is to use a simple and efficient hot-pressing assisted synthesis method to prepare a green lignin adhesive with ultra-high lignin content, excellent bonding properties and good thermal stability through the condensation process of lignin under high temperature conditions, thereby giving plywood excellent strength. Summary of the invention
[0005] The object of the present invention is to provide a lignin-based wood board adhesive and a preparation method thereof. The wood board adhesive has an ultra-high lignin content, good adhesion performance and thermal stability. The plywood prepared using the wood board adhesive has excellent tensile and compressive properties. The preparation method is simple and easy to mass produce.
[0006] The present invention provides a method for preparing a wood board adhesive by hydrothermal assisted synthesis, which utilizes the repolymerization of lignin in a hydrothermal environment. The specific steps are as follows: (1) dissolving lignin in an alkaline solution; (2) adding a cross-linking agent and mixing evenly, and standing for a period of time; (3) applying the above pre-cross-linking liquid evenly on the bonding surface of the veneer; (4) combining the veneers and hot pressing to obtain a plywood.
[0007] The concentration of the lignin in the alkaline solution is 100 to 500 g / L;
[0008] The mass ratio of the cross-linking agent to lignin is 20 to 200 g / L;
[0009] The alkaline pH range is 12 to 14;
[0010] The standing time ranges from 0.5 to 2 hours;
[0011] The coating amount ranges from 50 to 200 g / m 2 ;
[0012] The initial pressure increase is to 1.25 MPa;
[0013] The lignin includes sulfate lignin, alkali lignin, hydrolyzed lignin, enzymatic lignin, and organic solvent lignin obtained from different raw materials through different treatment methods. The different raw materials include woody plants, herbaceous plants, and vascular plants. The different treatment methods include acid, alkali, supercritical, two-phase aqueous, ionic liquid, organic solvent, and enzyme treatment.
[0014] The alkaline solution is one of sodium hydroxide, potassium hydroxide, calcium hydroxide and ammonia solution with different concentrations.
[0015] The cross-linking agent is one or more glycidyl ether cross-linking agents with different molecular weights.
[0016] The advantages and features of the present invention are:
[0017] The present invention utilizes a hydrothermal assisted synthesis method to cause lignin to repolymerize under a hydrothermal environment. The method is simple, efficient, and easy to carry out large-scale production.
[0018] The lignin-based wood board adhesive prepared by the invention has an ultra-high lignin content (85wt%) and excellent wood board bonding performance.
[0019] The self-condensation of lignin subunits during the synthesis of wood board adhesives can significantly increase the degree of cross-linking of lignin materials, thereby reducing the addition of toxic cross-linking agents. DETAILED DESCRIPTION
[0020] The inventors of the present invention, through in-depth research, prepared a lignin-based wood board adhesive for the first time using a hydrothermal-assisted synthesis method.
[0021] In order to more clearly understand the technical content of the present invention, the following embodiments are used for detailed description, the purpose of which is to better understand the content of the present invention rather than to limit the protection scope of the present invention.
[0022] Example 1
[0023] A 0.3 g / mL lignin solution was prepared with 1 mol / L KOH. After adding a certain amount of ethylene glycol diglycidyl ether crosslinking agent (solid content of 15 wt%), the solution system was mixed at room temperature (25°C) for 1 hour to obtain a lignin-based wood board adhesive. Poplar veneer (100×100×2 mm) was used, and the adhesive was evenly applied to the bonding surface of the veneer according to GB / T 17657-2013, with an adhesive amount of 85±5 g / m on each side. The obtained veneer was assembled on the heating plate of a hot press, pre-pressed for 5 seconds under the conditions of a hot pressing pressure of 2.0 MPa and a hot pressing temperature of 100°C, and the pressure was maintained for 5 minutes to obtain plywood 1.
[0024] Example 2
[0025] A 0.3 g / mL lignin solution was prepared with 1 mol / L KOH. After adding a certain amount of ethylene glycol diglycidyl ether crosslinking agent (solid content of 15 wt%), the solution system was mixed at room temperature (25°C) for 1 hour to obtain a lignin-based wood board adhesive. Poplar veneer (100×100×2 mm) was used, and the adhesive was evenly applied to the bonding surface of the veneer according to GB / T 17657-2013, with an adhesive amount of 85±5 g / m on each side. The obtained veneer was assembled on the heating plate of the hot press, pre-pressed for 5 seconds under the conditions of hot pressing pressure of 2.0 MPa and hot pressing temperature of 120°C, and the pressure was maintained for 5 minutes to obtain plywood 2.
[0026] Example 3
[0027] A 0.3 g / mL lignin solution was prepared with 1 mol / L KOH. After adding a certain amount of ethylene glycol diglycidyl ether crosslinker (solid content of 15 wt%), the solution system was mixed at room temperature (25°C) for 1 hour to obtain a lignin-based wood board adhesive. Poplar veneer (100×100×2 mm) was used, and the adhesive was evenly applied to the bonding surface of the veneer according to GB / T 17657-2013, with an adhesive coating amount of 85±5 g / m on each side. The obtained veneer was assembled on the heating plate of the hot press, pre-pressed for 5 seconds under the conditions of hot pressing pressure of 2.0 MPa and hot pressing temperature of 140°C, and maintained for 5 minutes to obtain plywood 3.
[0028] Example 4
[0029] A 0.3 g / mL lignin solution was prepared with 1 mol / L KOH. After adding a certain amount of ethylene glycol diglycidyl ether crosslinker (solid content of 15 wt%), the solution system was mixed at room temperature (25 ° C) for 1 hour to obtain a lignin-based wood board adhesive. Poplar veneer (100 × 100 × 2 mm) was used, and the adhesive was evenly applied to the bonding surface of the veneer according to GB / T 17657-2013, with an adhesive amount of 85 ± 5 g / m on each side. The obtained veneer was combined on the heating plate of the hot press, pre-pressed for 5 seconds under the conditions of hot pressing pressure of 2.0 MPa and hot pressing temperature of 160 ° C, and the pressure was maintained for 5 minutes to obtain plywood 4.
[0030] Example 5
[0031] A 0.3 g / mL lignin solution was prepared with 1 mol / L KOH. After adding a certain amount of ethylene glycol diglycidyl ether crosslinker (solid content of 15 wt%), the solution system was mixed at room temperature (25 ° C) for 1 hour to obtain a lignin-based wood board adhesive. Poplar veneer (100 × 100 × 2 mm) was used, and the adhesive was evenly applied to the bonding surface of the veneer according to GB / T 17657-2013, with an adhesive amount of 85 ± 5 g / m on each side. The obtained veneer was assembled on the heating plate of the hot press, pre-pressed for 5 seconds under the conditions of hot pressing pressure of 2.0 MPa and hot pressing temperature of 180 ° C, and the pressure was maintained for 5 minutes to obtain plywood 5.
[0032] Plywood Strength Test
[0033] The dry bonding strength and wet bonding strength of plywood are tested using the method specified in GB / T 17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels".
[0034] Table 1 Test results of bonding strength of plywood
[0035]
Claims
1. A method for preparing plywood based on a high lignin content adhesive, characterized in that: The following steps are involved: (1) dissolving lignin in an alkaline solution; (2) adding a cross-linking agent and mixing evenly, and letting it stand for a while; (3) applying the pre-crosslinking liquid evenly on the bonding surface of the veneer; (4) Combining and hot pressing the veneers to obtain plywood; The concentration of the lignin in the alkaline solution is 100 to 500 g / L; The mass ratio of the cross-linking agent to lignin is 20 to 200 g / L; The alkaline pH range is 12 to 14; The standing time ranges from 0.5 to 2 hours; The coating amount ranges from 50 to 200 g / m 2 The initial pressure increase is to 1.25 MPa.
2. The method according to claim 1, characterized in that The lignin includes sulfate lignin, alkali lignin, hydrolyzed lignin, enzymatic lignin, and organic solvent lignin obtained from different raw materials through different treatment methods. The different raw materials include woody plants, herbaceous plants, and vascular plants. The different treatment methods include acid, alkali, supercritical, two-phase aqueous, ionic liquid, organic solvent, and enzyme treatment.
3. The method according to claim 1, characterized in that The alkaline solution is one of sodium hydroxide, potassium hydroxide, calcium hydroxide and ammonia solution with different concentrations.
4. The method according to claim 1, characterized in that: The cross-linking agent is one or more glycidyl ether cross-linking agents with different molecular weights.
Citation Information
Patent Citations
Method for improving mechanical property of lignin-based adhesive plywood
CN109093786A
High-strength full-degradable lignin-based super absorbent resin and preparation method thereof
CN112048081A
Process for preparing bonding resin
CN114008168A
Lignin-based adhesive
CN115558466A
Cited By
Lignin-epoxidized carboxymethyl chitosan adhesive as well as preparation method and application thereof
CN122563545A