Composite metal oxide magnesium-based material as well as preparation method and application thereof

By preparing composite metal oxide magnesium-based materials, the special morphology and high specific surface area of ​​prism CeO2 are used to optimize the microstructure of magnesium-based materials, and the problems of slow kinetics and high temperature during hydrogen absorption and discharge are solved. , achieved significant performance improvement and improved cycle stability, providing efficient and safe solutions for hydrogen energy storage.

CN118929575AActive Publication Date: 2024-11-12STATE PWR INVT CORP SHAANXI NEW ENERGY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411158965.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

During the hydrogen absorption and release process, magnesium-based materials have problems such as slow hydrogen absorption and release kinetics, high hydrogen absorption and release temperature and poor cycle stability, which limits their practical application.

Method used

The prismatic CeO2 was prepared by hydrothermal method using composite metal oxide magnesium-based material, and ball milling was performed during mechanical alloying to form MgH2-CeO2 (prism-shaped) material, and the special morphology of CeO2 and high specific surface area were used to optimize the material. The microstructure of the microstructure improves its hydrogen storage performance.

Benefits of technology

It significantly improves the dynamic performance of hydrogen absorption and release, reduces the hydrogen absorption and release temperature, enhances cycle stability and hydrogen storage capacity, and provides an efficient and safe hydrogen energy storage solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929575A_ABST
    Figure CN118929575A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a composite metal oxide magnesium-based material. The preparation method comprises the following steps: step 1, taking cerium nitrate hexahydrate (Ce (NO3) 3.6 H2O) and urea as raw materials, adding an aqueous solution of the cerium nitrate hexahydrate (Ce (NO3) 3.6 H2O) and the urea into a stainless steel high-pressure sterilizer with a polytetrafluoroethylene lining, then sealing, and carrying out hydrothermal synthesis; filtering the precipitate, then washing the precipitate with deionized water to obtain a CeO2 material, and roasting the obtained CeO2 material in air to obtain prismatic CeO2; 2, metal magnesium powder with the purity larger than or equal to 99.8% and the prismatic CeO2 prepared in the first step are selected, weighed in a glove box and then put into a high-energy ball milling tank for ball milling; and finally, Mg-CeO2 is obtained. And step 3, putting the Mg-CeO2 obtained in the step 2 into a hydrogenation kettle in an inert atmosphere, so as to obtain MgH2-CeO2. The size of the finally generated composite magnesium-based material can be greatly reduced, and the hydrogen storage performance of the material is improved by optimizing the microstructure and composition of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogen storage materials, and in particular relates to a composite metal oxide magnesium-based material, a preparation method and an application thereof. Background Art

[0002] With the continuous growth of global energy demand and the increasing prominence of environmental problems, the development and utilization of clean energy has become a key issue that needs to be solved urgently. Hydrogen energy has gradually attracted widespread attention due to its advantages such as zero emissions, high energy density and renewability. However, the large-scale application of hydrogen energy still faces the technical bottleneck of efficient storage and transportation of hydrogen. At present, hydrogen storage methods mainly include high-pressure gas storage, low-temperature liquid storage and solid-state hydrogen storage. Among them, although high-pressure gaseous hydrogen storage and low-temperature liquid hydrogen storage are relatively mature technologies, they have shortcomings such as safety issues, high energy consumption and limited storage density. In contrast, solid-state hydrogen storage has become a hot research area due to its high hydrogen storage density and good safety.

[0003] Among solid-state hydrogen storage materials, magnesium-based hydrides are one of them, which are favored due to their abundant resources, high hydrogen storage capacity and good safety. However, magnesium-based materials have problems such as slow hydrogen absorption and desorption kinetics, high hydrogen absorption and desorption temperature and poor cycle stability during the hydrogen absorption and desorption process, which limit their practical application.

[0004] To solve these problems, researchers have proposed a variety of modification strategies, among which metal oxide composite modification is an effective method. NSMustafa et al. (10.1016 / j.jallcom.2016.11.158) studied the hydrogen absorption and desorption properties of CeO2 doped with MgH2, but the microstructure of the material was not optimized enough, and the interface effect and nano effect of CeO2 were not fully utilized.

[0005] In summary, the existing magnesium-based materials have the problems of slow hydrogen absorption and desorption kinetics, high hydrogen absorption and desorption temperature and poor cycle stability during the hydrogen absorption and desorption process. Summary of the invention

[0006] In order to overcome the above problems existing in the prior art, the purpose of the present invention is to provide a composite metal oxide magnesium-based material, a preparation method and an application thereof. The prismatic CeO2 ball milling of the composite metal oxide magnesium-based material with a special morphology can greatly reduce the size of the final composite magnesium-based material, and improve its hydrogen storage performance by optimizing the microstructure and composition of the material.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A composite metal oxide magnesium-based material, namely MgH2-CeO2 (prismatic), wherein the content of Mg is 90-95wt.%, the content of CeO2 is 5-10wt.%, and the specific surface area of ​​prismatic CeO2 is 77.682m 2 / g, the size of prismatic CeO2 is 200~550nm.

[0009] The prismatic CeO2 is formed by nucleation and condensation of 30-600nm cerium particles over time in a hydrothermal process. The thickness of the prism is about 200-300nm and the side length is about 200-550nm. During the mechanical mixing process, due to the hard texture of the oxide, it impacts and collides with the grinding balls during ball milling, resulting in repeated cold welding and fracture, which is more conducive to grain refinement and inhibition of agglomeration effect than ordinary CeO2.

[0010] A method for preparing a composite metal oxide magnesium-based material comprises the following steps:

[0011] Step 1: Preparation of prismatic CeO2:

[0012] Using cerium nitrate hexahydrate (Ce(NO3)3·6H2O) and urea as raw materials, the aqueous solution of cerium nitrate hexahydrate (Ce(NO3)3·6H2O) and urea was added into a polytetrafluoroethylene-lined stainless steel autoclave, which was then sealed for hydrothermal synthesis;

[0013] The precipitate is filtered and then washed with deionized water to obtain a CeO2 material, and the obtained CeO2 material is calcined in air to obtain a prismatic CeO2;

[0014] The hydrothermal method for preparing CeO2 with special morphology mainly uses urea as a precipitant and cerium nitrate hexahydrate (Ce(NO3)3·6H2O) as a metal precursor solution. The acidity and alkalinity of the solution are changed by changing the urea concentration, thereby affecting the nucleation process of the material. The higher hydrothermal temperature promotes the hydration product to generate CeO2 through a dissolution-recrystallization mechanism.

[0015] Step 2: Mechanical alloying modification:

[0016] Selecting magnesium powder with a purity of ≥99.8% and prismatic CeO2 prepared in step 1, weighing them in a glove box and then putting them into a high-energy ball mill for ball milling; finally obtaining Mg-CeO2 (prismatic);

[0017] Step 3: Preparation of MgH2-CeO2 (prismatic):

[0018] The Mg-CeO2 (prism-shaped) obtained in step 2 is placed in a hydrogenation reactor under an inert atmosphere to obtain MgH2-CeO2 (prism-shaped).

[0019] In step 1, the conditions of hydrothermal synthesis are as follows: synthesis time is 2-24h; synthesis temperature is 120-180°C; urea concentration is 0.0375-0.15g / mL; Ce(NO3)3·6H2O concentration is 0.025-0.25g / mL.

[0020] The obtained CeO2 material is calcined in air at 400-600°C for 2-4h.

[0021] In the step 2, Mg:CeO2=9:1, and the ball-to-material ratio of ball milling is 40:1-30:1; first, the ball milling jar is rinsed 2-3 times under 0.2MPa hydrogen pressure, and then placed in a ball mill after being pressurized at 0.4-0.5MPa, and rotated at 600-1000rpm, forward for 5min, rest for 5min, reverse for 5min, rest for 5min, cycle for 20min, and last for 10-12h. During this period, the ball milling jar is gasified once every 2h, and finally Mg-CeO2 (prismatic) is obtained, and its final average particle size d 50 =1.26μm, d 90 =2.78μm.

[0022] In the step 2, after high-energy ball milling and mechanical alloying, the powder size of the composite metal oxide magnesium-based hydrogen storage material after screening is ≤2.78 μm.

[0023] In the step 3, the cavity is cleaned 2-3 times with hydrogen at a hydrogen pressure of 0.2 MPa before heating, and the temperature is increased at a hydrogen pressure of 2-4 MPa, with an average heating rate of 5-10°C / min, and the temperature is increased to 300-380°C, the hydrogen pressure is 4-6 MPa, and the temperature is kept for 8-10 hours. After the reaction is completed, the cavity is cooled to room temperature with the furnace.

[0024] In step 3, during the mechanical alloying modification process in step 2, the long-term high-speed ball milling in hydrogen atmosphere will reduce a small amount of Ce on the obtained Mg-CeO2, and after step 3, a small amount of CeH2 will be in situ generated on the obtained MgH2-CeO2 (prismatic). 2.73 .

[0025] The composite metal oxide magnesium-based material is used for hydrogen storage, with the composite metal oxide magnesium-based material as the hydrogen storage material and the metal oxide CeO2 as a catalyst. During the process of hydrogen absorption and desorption, the high-valent metal in the metal oxide will be reduced to a low-valent state, thereby forming a diffusion channel for hydrogen atoms. During the addition process, mechanical alloying can introduce various defects such as vacancies, dislocations and stacking faults, thereby increasing the free energy of the magnesium-based hydrogen storage material and further improving the hydrogen absorption and desorption kinetics of the magnesium-based hydrogen storage material.

[0026] In the process of hydrogen absorption, hydrogen molecules are first adsorbed on the surface of the material and dissociated into hydrogen atoms. High-valent metal ions in metal oxides, such as Ce,4+ When it comes into contact with hydrogen, it will undergo a reduction reaction and be reduced to a low-valent metal ion Ce 3 + This reduction process releases oxygen vacancies or defect sites, forming channels for hydrogen atom diffusion inside the material. The diffusion channels form a "network" inside the material, making it easier for hydrogen atoms to move inside the material, thereby accelerating the diffusion of hydrogen inside the material. This mechanism significantly increases the hydrogen absorption rate of the material.

[0027] In the entire material preparation process, mechanical alloying is a commonly used method. Mechanical alloying uses mechanical means such as high-energy ball milling to fully mix metallic magnesium and metal oxides at the nanoscale. This process not only physically combines the two substances, but also introduces a large number of lattice defects such as vacancies, dislocations, and stacking faults into the material. The presence of these defects increases the free energy of the material, allowing hydrogen atoms to more easily overcome the energy barriers in the process of hydrogen absorption and desorption, thereby accelerating the hydrogen absorption and desorption process. In addition, these defects can also serve as capture points for hydrogen atoms, further enhancing the hydrogen storage capacity of the material.

[0028] Composite metal oxide magnesium-based materials have broad application prospects in hydrogen fuel cells, solid-state hydrogen storage devices and renewable energy storage, providing an efficient and safe solution for the future development and utilization of hydrogen energy.

[0029] Beneficial effects of the present invention:

[0030] First: Prismatic CeO2 as a catalyst is hard in the mechanical alloying process due to its special prismatic morphology. It is helpful for grinding and adheres to the gradually refined Mg particles during the grinding process to separate the magnesium particles, which has excellent refining effect and inhibits the agglomeration effect. Through the ball milling of CeO2 with special prismatic morphology, the size of the final composite magnesium-based material can be greatly reduced. After ball milling, the average particle size of the magnesium-based composite material is d 50 About 1.26 μm, d 90 It is about 2.78μm, and the preparation process is simple and the operation process is concise.

[0031] Second: In the process of mechanical alloying, metal oxide CeO2 is introduced to form a trace amount of CeH in the final material. 2.73 , forming a "hydrogen pump" effect with MgH2, which is beneficial to the thermodynamics of hydrogen absorption and desorption. Part of CeO2 is embedded in the surface of the Mg matrix during ball milling, providing an auxiliary diffusion channel for hydrogen.

[0032] Third: Formation of CeH 2.73This reduces the energy barrier of the hydrogen storage material, thereby reducing the apparent activation energy of the hydrogen absorption / desorption reaction of the magnesium-based hydrogen storage material and improving its hydrogen storage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The SEM image and XRD diffraction pattern of the prepared prismatic CeO2.

[0034] Figure 2 This is a statistical chart of the particle size of the magnesium-based hydrogen storage material after alloying for 12 hours.

[0035] Figure 3 These are the SEM images and XRD diffraction patterns of composite metal oxide magnesium-based hydrogen storage materials. DETAILED DESCRIPTION

[0036] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0037] Example 1

[0038] Select metal magnesium powder with a purity of ≥99.98% and prepared prismatic CeO2, weigh 1.8 g of Mg powder and 0.2 g of prismatic CeO2 in an inert gas, and put them into a high-energy ball mill with a ball-to-material ratio of 30:1. The ball mill was rinsed with hydrogen 2-3 times at 0.2MPa hydrogen pressure, and then pressurized at 0.4MPa hydrogen pressure and placed in a ball mill. The mill was rotated at 600 rpm, with a forward rotation of 5min, a rest of 5min, a reverse rotation of 5min, a rest of 5min, a cycle of 20min, and a duration of 12h. During this period, the ball mill was replenished with gas once every 2h. The Mg-CeO2 (prismatic) obtained was placed in a hydrogenation reactor under an inert atmosphere. The cavity was cleaned with hydrogen at 0.2MPa hydrogen pressure for 2-3 times before heating. The temperature was increased at a hydrogen pressure of 2MPa, with an average heating rate of 5℃ / min, and the temperature was increased to 300℃, with a hydrogen pressure of 4MPa, and the temperature was kept for 8h. After the reaction was completed, the MgH2-CeO2 (prismatic) was obtained by cooling to room temperature with the furnace. The average size D 90 =2.73μm.

[0039] The results show that the material shows significant performance improvement in the process of hydrogen absorption and desorption. Compared with pure MgH2 material without CeO2 doping, the hydrogen absorption and desorption kinetics are greatly improved, the hydrogen absorption and desorption temperature is significantly reduced, and it has excellent cycle stability and high hydrogen storage capacity. This shows that the prepared MgH2-CeO2 (prismatic) material has broad application prospects in hydrogen energy storage applications.

[0040] Example 2

[0041] Select metal magnesium powder with a purity of ≥99.98% and prepared prismatic CeO2, weigh 0.95g of Mg powder and 0.05g of prismatic CeO2 in an inert gas, and put them into a high-energy ball mill with a ball-to-material ratio of 35:1. The ball mill is rinsed with hydrogen 2-3 times at a hydrogen pressure of 0.2MPa, and then pressurized at a hydrogen pressure of 0.45MPa and placed in a ball mill at a speed of 900rpm, with forward rotation for 5min, pause for 5min, reverse rotation for 5min, pause for 5min, and a cycle of 20min for 12h. During this period, the ball mill is replenished with gas once every 2h. The finally obtained Mg-CeO2 (prismatic) is placed in a hydrogenation kettle under an inert atmosphere, and the cavity is cleaned 2-3 times with hydrogen at a hydrogen pressure of 0.2MPa before heating. The temperature is increased at a hydrogen pressure of 2MPa with an average heating rate of 8℃ / min to 350℃, a hydrogen pressure of 5MPa, and insulation for 9h. Then, it is cooled to room temperature with the furnace to obtain MgH2-CeO2 (prismatic).

[0042] The results show that the material shows significant performance improvement in the process of hydrogen absorption and desorption. Compared with pure MgH2 material without CeO2 doping, the hydrogen absorption and desorption kinetics are greatly improved, the hydrogen absorption and desorption temperature is significantly reduced, and it has excellent cycle stability and high hydrogen storage capacity. This shows that the prepared MgH2-CeO2 (prismatic) material has broad application prospects in hydrogen energy storage applications.

[0043] Example 3

[0044] Metal magnesium powder with a purity of ≥99.98% and prepared prismatic CeO2 were selected, 2.76 g of Mg powder and 0.24 g of prismatic CeO2 were weighed in a glove box, and then loaded into a high-energy ball mill with a ball-to-material ratio of 40:1. The ball mill is rinsed with hydrogen 2-3 times at a hydrogen pressure of 0.2MPa, and then pressurized at a hydrogen pressure of 0.5MPa and placed in a ball mill at a speed of 1000rpm, with forward rotation for 5min, pause for 5min, reverse rotation for 5min, pause for 5min, and a cycle of 20min for 12h. During this period, the ball mill is replenished with gas once every 2h. The finally obtained Mg-CeO2 (prismatic) is placed in a hydrogenation kettle under an inert atmosphere, and the cavity is cleaned 2-3 times with hydrogen at a hydrogen pressure of 0.2MPa before heating. The temperature is increased at a hydrogen pressure of 2MPa, with an average heating rate of 10℃ / min, the temperature is increased to 380℃, the hydrogen pressure is 6MPa, and the temperature is kept for 10h. Then, it is cooled to room temperature with the furnace to obtain MgH2-CeO2 (prismatic).

[0045] The results show that the material shows significant performance improvement in the process of hydrogen absorption and desorption. Compared with pure MgH2 material without CeO2 doping, the hydrogen absorption and desorption kinetics are greatly improved, the hydrogen absorption and desorption temperature is significantly reduced, and it has excellent cycle stability and high hydrogen storage capacity. This shows that the prepared MgH2-CeO2 (prismatic) material has broad application prospects in hydrogen energy storage applications.

[0046] like Figure 1 The SEM image and XRD diffraction image of the prismatic CeO2 prepared by the present invention are shown. From the XRD diffraction image, it can be seen that the prepared prismatic CeO2 basically meets the peak value correspondence of PDF card No. 16-4225. It can be clearly seen from the SEM image that the prismatic CeO2 has a triangular prism shape with a size between 300-500nm.

[0047] like Figure 2 The figure shows the average particle size statistics of Mg-xCeO2 (x = 5% - 10%) material after mechanical alloying for 12 hours. It can be seen that the final average particle size d 50 =1.26μm, d 90 =2.78μm, basically achieving the purpose of refining MgH2.

[0048] like Figure 3 The SEM image and XRD diffraction pattern of the final prepared MgH2-xCeO2 (x = 5% -10%) are shown. From the XRD diffraction pattern, it can be seen that MgH2 and a very small amount of CeH 2.73 , which shows that CeH 2.73 With the presence of MgH2.

[0049] In the present invention, mechanical alloying is a solid-state reaction in which metal and alloy powders are subjected to repeated cold welding and fracture by impact and collision with grinding balls in a high-energy ball mill under oxygen-free conditions to obtain alloyed powders. Through this reaction, a second phase such as CeH 2.73 , thereby reducing the activation energy of hydrogen absorption and desorption, and improving thermodynamics. In addition, mechanical alloying is carried out in a hydrogen atmosphere, and hydrogen can serve as a protective atmosphere and also as a pre-hydrogenation. After adding CeO2, during the mechanical alloying process, on the one hand, due to its hard oxide texture, it helps with grinding, and during the grinding process, it adheres to the gradually refined Mg particles, separating the magnesium particles, which plays a role in refining the grains and inhibiting the agglomeration effect. On the other hand, during the high-energy ball milling process, CeO2 can in-situ reduce trace amounts of CeH on Mg in a hydrogen atmosphere. 2.73 The "hydrogen pump" effect formed by it and MgH2 is more conducive to the kinetics of hydrogen absorption and desorption.

[0050] The present invention optimizes the preparation method and mechanical alloying process of CeO2 to form a prismatic CeO2 structure, and utilizes its high specific surface area and special morphology to improve the hydrogen absorption and desorption performance of magnesium-based materials. In addition, by optimizing the ball milling and hydrogenation process, the hydrogen storage capacity and cycle stability of the material are further improved.

Claims

1. A composite metal oxide magnesium-based material, namely MgH2-CeO2 (prismatic), wherein the content of Mg is 90-95wt.%, the content of CeO2 is 5-10wt.%, and the specific surface area of ​​prismatic CeO2 is 77.682m 2 / g, the size of prismatic CeO2 is 200~550nm.

2. A composite metal oxide magnesium-based material according to claim 1, characterized in that: The prismatic CeO2 is formed by nucleation and condensation of cerium particles of 30-600 nm over time during a hydrothermal process. The thickness of the prism is about 200-300 nm, and the side length is about 200-550 nm.

3. A method for preparing a composite metal oxide magnesium-based material according to claim 1 or 2, characterized in that: The steps include: Step 1: Preparation of prismatic CeO2: Using cerium nitrate hexahydrate (Ce(NO3)3·6H2O) and urea as raw materials, the aqueous solution of cerium nitrate hexahydrate (Ce(NO3)3·6H2O) and urea was added into a polytetrafluoroethylene-lined stainless steel autoclave, which was then sealed for hydrothermal synthesis; The precipitate is filtered and then washed with deionized water to obtain a CeO2 material, and the obtained CeO2 material is calcined in air to obtain a prismatic CeO2; Step 2: Mechanical alloying modification: Selecting magnesium powder with a purity of ≥99.8% and prismatic CeO2 prepared in step 1, weighing them in a glove box and then putting them into a high-energy ball mill for ball milling; finally obtaining Mg-CeO2 (prismatic); Step 3: Preparation of MgH2-CeO2 (prismatic): The Mg-CeO2 (prism-shaped) obtained in step 2 is placed in a hydrogenation reactor under an inert atmosphere to obtain MgH2-CeO2 (prism-shaped).

4. The method for preparing a composite metal oxide magnesium-based material according to claim 3, characterized in that: In step 1, the conditions of hydrothermal synthesis are as follows: synthesis time is 2-24h; synthesis temperature is 120-180°C; urea concentration is 0.0375-0.15g / mL; Ce(NO3)3·6H2O concentration is 0.025-0.25g / mL; The obtained CeO2 material is calcined in air at 400-600°C for 2-4h.

5. The method for preparing a composite metal oxide magnesium-based material according to claim 3, characterized in that: In the step 2, Mg:CeO2=9:1, and the ball-to-material ratio of ball milling is 40:1-30:1; first, the ball milling jar is rinsed 2-3 times under 0.2MPa hydrogen pressure, and then placed in a ball mill after being pressurized at 0.4-0.5MPa, and rotated at 600-1000rpm, forward for 5min, rest for 5min, reverse for 5min, rest for 5min, cycle for 20min, and last for 10-12h. During this period, the ball milling jar is gasified once every 2h, and finally Mg-CeO2 (prismatic) is obtained, and its final average particle size d 50 =1.26μm, d 90 =2.78μm.

6. The method for preparing a composite metal oxide magnesium-based material according to claim 3, characterized in that: In the step 2, after high-energy ball milling and mechanical alloying, the powder size of the composite metal oxide magnesium-based hydrogen storage material after screening is ≤2.78 μm.

7. The method for preparing a composite metal oxide magnesium-based material according to claim 3, characterized in that: In the step 3, the cavity is cleaned 2-3 times with hydrogen at a hydrogen pressure of 0.2 MPa before heating, and the temperature is increased at a hydrogen pressure of 2-4 MPa, with an average heating rate of 5-10°C / min, and the temperature is increased to 300-380°C, the hydrogen pressure is 4-6 MPa, and the temperature is kept for 8-10 hours. After the reaction is completed, the cavity is cooled to room temperature with the furnace.

8. The method for preparing a composite metal oxide magnesium-based material according to claim 3, characterized in that: In step 3, during the mechanical alloying modification process in step 2, the long-term high-speed ball milling in hydrogen atmosphere will reduce a small amount of Ce on the obtained Mg-CeO2, and after step 3, a small amount of CeH2 will be in situ generated on the obtained MgH2-CeO2 (prismatic). 2.73 .

9. The use of the composite metal oxide magnesium-based material according to any one of claims 1 to 8, characterized in that: The composite metal oxide magnesium-based material is used for hydrogen storage, with the composite metal oxide magnesium-based material as the hydrogen storage material and the metal oxide CeO2 as a catalyst. During the process of hydrogen absorption and desorption, the high-valent metal in the metal oxide will be reduced to a low-valent state, thereby forming a diffusion channel for hydrogen atoms. During the addition process, mechanical alloying can introduce various defects such as vacancies, dislocations and stacking faults, thereby increasing the free energy of the magnesium-based hydrogen storage material and further improving the hydrogen absorption and desorption kinetics of the magnesium-based hydrogen storage material.

10. The use of the composite metal oxide magnesium-based material according to claim 9, characterized in that: In the process of hydrogen absorption, hydrogen molecules are first adsorbed on the surface of the material and dissociated into hydrogen atoms. High-valent metal ions in metal oxides, such as Ce, 4+ When it comes into contact with hydrogen, it will undergo a reduction reaction and be reduced to a low-valent metal ion Ce 3+ This reduction process releases oxygen vacancies or defect sites, forming channels for hydrogen atom diffusion inside the material. The diffusion channels form a "network" inside the material, making it easier for hydrogen atoms to move inside the material, thereby accelerating the diffusion of hydrogen inside the material. This mechanism significantly increases the hydrogen absorption rate of the material.

Citation Information

Patent Citations

  • Mg-based hydrogen storage material with metal oxide added and preparation method of Mg-based hydrogen storage material

    CN102862958A

  • Preparation method of triangular prism-shape ceric oxide

    CN102992384A

  • Magnesium-based hydrogen storage material and preparation method thereof

    CN103526141A

  • Preparation method of metal oxide composite magnesium hydride hydrogen storage material

    CN110980635A

  • Bimetal composite rodlike nano-catalyst and application thereof in C-H bond oxidation reaction

    CN114345332A