Preparation method of electronic grade sulfuric acid
By using fiber microporous membrane filtration and absorption technology, the problem of difficult removal of impurities in industrial sulfur trioxide is solved, and the preparation of high-purity electronic grade sulfuric acid is realized, the process flow is simplified, energy consumption and cost are reduced, and product quality is ensured.
Patent Information
- Application Number
- CN202310523251.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-10
AI Technical Summary
In the prior art, particulate matter and impurities such as sulfur dioxide contained in industrial sulfur trioxide are difficult to effectively remove, resulting in complex preparation process of electronic-grade sulfuric acid, high cost, high energy consumption, and dangerous waste gases.
Filtration and absorption by fiber microporous membranes. The fiber microporous membrane made of a mixture of fluoropolymers and polyethylene glycol can simultaneously filter and remove particulate impurities and absorb sulfur dioxide, simplify the process flow and reduce risks. Chemical use.
The preparation of high-purity electronic grade sulfuric acid is realized, the energy consumption and raw material cost of the device are reduced, the product quality is stable, the sulfur dioxide content is less than 1000ppb, the granular impurity content is less than 50 pieces/mL, and the single metal cation content is less than 100ppt.
Smart Images

Figure BDA0004221785030000111 
Figure BDA0004221785030000121 
Figure BDA0004221785030000122
Abstract
Description
Technical Field
[0001] The invention relates to the field of electronic chemicals, and in particular to a method for preparing electronic-grade sulfuric acid. Background Art
[0002] Electronic grade sulfuric acid is an ultra-clean, high-purity reagent that is often used in microelectronics technology for cleaning silicon wafers, photolithography, corrosion, and corrosion and electroplating cleaning of printed circuit boards. Impurities in electronic grade chemicals can seriously affect the reliability and completion of semiconductor equipment manufacturing.
[0003] The gas absorption method is commonly used in industry, that is, ultrapure water or ultrapure sulfuric acid is used to absorb sulfur trioxide to prepare ultrapure sulfuric acid, but industrial sulfur trioxide contains a certain amount of impurities such as particulate matter and sulfur dioxide. In the prior art, it is usually purified by adding oxidants, air stripping, evaporation purification, multi-stage filtration and other methods. The system is complex, the raw material cost is high, the energy consumption is high, and the waste gas generated by the stripping will also increase the cost of the three wastes treatment.
[0004] Therefore, there is an urgent need for a method for refining high-purity electronic-grade sulfuric acid with simple equipment, no stripping waste gas, and the ability to effectively remove impurities in the raw materials. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem of difficulty in removing impurities such as particulate matter and sulfur dioxide contained in industrial sulfur trioxide in the prior art, and to provide a method for preparing electronic-grade sulfuric acid. The method adopts a fiber microporous membrane that has the function of filtering and removing particulate impurities and absorbing and removing sulfur dioxide, and can effectively remove sulfur dioxide and particulate impurities in the raw materials to obtain electronic-grade sulfuric acid with stable product quality.
[0006] In order to achieve the above object, the present invention provides a method for preparing electronic grade sulfuric acid, the preparation method comprising the following steps:
[0007] (1) vaporizing crude sulfur trioxide to obtain a gaseous sulfur trioxide raw material;
[0008] (2) filtering and absorbing the gaseous sulfur trioxide raw material and ultrapure water through a fiber microporous membrane to obtain a semi-finished sulfuric acid solution;
[0009] (3) concentrating the semi-finished sulfuric acid solution to obtain an electronic grade sulfuric acid crude product;
[0010] (4) cooling and filtering the crude electronic-grade sulfuric acid to obtain the electronic-grade sulfuric acid;
[0011] The fiber microporous membrane is prepared by granulating, spinning, winding and stretching a mixture of fluorine-containing polymer and polyethylene glycol.
[0012] Through the above technical solution, the beneficial effects of the present invention are:
[0013] The present invention adopts industrial sulfur trioxide as raw material, and after vaporization, it is filtered and absorbed by a fiber microporous membrane filter. Polyethylene glycol (PEG) contained in the fiber microporous membrane has a selective adsorption effect on sulfur dioxide, and the addition of PEG causes dense pores to be generated on the outer surface and inside of the fiber, thereby increasing the specific surface area of the fiber microporous membrane and ensuring the mechanical strength of the membrane. Therefore, the fiber microporous membrane can not only filter and remove particulate impurities, but also the hollow structure of the fiber microporous membrane can effectively absorb and remove sulfur dioxide. Compared with the prior art, the method can filter and remove particulate impurities and remove sulfur dioxide at the same time, without the need to use desulfurization liquid, and without the need to use hydrogen peroxide or ozone for gas stripping, is easy to operate, reduces the introduction of hazardous chemicals, can effectively reduce the material consumption and energy consumption of the device, and can effectively remove sulfur dioxide and particulate impurities in the raw material, the product quality is stable, and can be used to produce high-purity electronic grade sulfuric acid with a sulfur dioxide content of less than 1000ppb, a particulate impurity content of less than or equal to 50 / mL, and a single metal cation content of less than 100ppt. DETAILED DESCRIPTION
[0014] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0015] The present invention provides a method for preparing electronic grade sulfuric acid, the preparation method comprising the following steps:
[0016] (1) vaporizing crude sulfur trioxide to obtain a gaseous sulfur trioxide raw material;
[0017] (2) filtering and absorbing the gaseous sulfur trioxide raw material and ultrapure water through a fiber microporous membrane to obtain a semi-finished sulfuric acid solution;
[0018] (3) concentrating the semi-finished sulfuric acid solution to obtain an electronic grade sulfuric acid crude product;
[0019] (4) cooling and filtering the crude electronic-grade sulfuric acid to obtain the electronic-grade sulfuric acid;
[0020] The fiber microporous membrane is prepared by granulating, spinning, winding and stretching a mixture of fluorine-containing polymer and polyethylene glycol.
[0021] In the present invention, industrial sulfur trioxide can be used as a raw material, which is filtered and absorbed by a fiber microporous membrane filter after vaporization. The fluorine-containing polymer in the fiber microporous membrane has excellent chemical corrosion resistance, high temperature resistance and oxidation resistance, as well as excellent flexibility, and has the characteristics of wear resistance and easy processing. It can withstand temperature changes or thermal shock conditions within the range of -29°C to 260°C for long-term normal use.
[0022] The fiber microporous membrane introduces hydrophilic groups by adding polyethylene glycol (PEG), which has an excellent removal effect on sulfur dioxide; in addition, the addition of PEG produces dense pores on the outer surface and inside of the fiber, increases the specific surface area and porosity of the fiber microporous membrane, increases the mass transfer channel, and enables the fiber microporous membrane to effectively filter and remove particulate impurities and sulfur dioxide, and has excellent separation efficiency. Therefore, the fiber microporous membrane is a dual-functional membrane that has the function of filtering and removing particulate impurities and absorbing and removing sulfur dioxide. After filtering and absorbing through the fiber microporous membrane filter, a semi-finished sulfuric acid solution after removing particulate impurities and sulfur dioxide is obtained, and then evaporated, concentrated, cooled and filtered to obtain electronic grade sulfuric acid that meets the standards. The prior art requires that the sulfur trioxide raw material be absorbed and filtered multiple times to obtain high-purity sulfur trioxide gas, and then reacted with pure water to prepare electronic grade sulfuric acid. Compared with the prior art, the method provided by the present invention has a simple device and is easy to operate, can effectively reduce the material and energy consumption of the device, and can effectively remove sulfur dioxide and particulate impurities in industrial sulfur trioxide raw materials through a fiber microporous membrane filter to obtain electronic grade sulfuric acid with stable product quality.
[0023] According to the present invention, in step (2), the gaseous sulfur trioxide raw material and ultrapure water pass through a fiber microporous membrane, the gaseous sulfur trioxide raw material is absorbed by the ultrapure water, and the obtained acidic liquid passes through the fiber microporous membrane. The fiber microporous membrane can filter and remove particulate impurities in the raw material, and can adsorb and remove sulfur dioxide in the gaseous sulfur trioxide raw material; the acidic liquid after removing the particulate impurities and sulfur dioxide is a semi-finished sulfuric acid solution.
[0024] According to the present invention, preferably, the method for preparing the fiber microporous membrane comprises the following steps: mixing the fluorine-containing polymer and polyethylene glycol, followed by granulation and spinning, and then winding and stretching.
[0025] According to a specific embodiment of the present invention, the preparation method of the fiber microporous membrane includes the following steps: mixing a fluorine-containing polymer and polyethylene glycol, and then granulating the granules, passing the obtained granules through a twin-screw spinning machine, and introducing nitrogen for spinning, after cooling and curing, winding into a membrane, and washing, drying and stretching.
[0026] According to the present invention, preferably, in the mixture, the amount of polyethylene glycol is 6-10wt% based on the weight of the fluorine-containing polymer. When the amount of polyethylene glycol meets this range, the porosity of the fiber microporous membrane can be fully improved while ensuring the mechanical strength of the fiber microporous membrane.
[0027] According to the present invention, preferably, the fluorine-containing polymer is selected from at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride, polyvinylidene fluoride, fluorinated ethylene-propylene copolymer, ethylene-tetrafluoroethylene copolymer (ETFE) and trifluorochloroethylene-ethylene copolymer, preferably polytetrafluoroethylene. Polytetrafluoroethylene has strong hydrophobicity, oxidation resistance, acid and alkali resistance and temperature resistance. After mixing it with polyethylene glycol, it is prepared into a fiber microporous membrane with a hollow structure, which can not only exert its super mechanical properties, have more excellent absorption and filtration capabilities, but also have a longer membrane service life.
[0028] According to the present invention, preferably, the weight average molecular weight of the fluoropolymer is 300,000-4,000,000 g / mol. The mixture of the fluoropolymer and polyethylene glycol is dispersed and stretched and spun to form microfibers, and the undeveloped parts are connected in the form of nodes, and such point lines are connected to form a microporous structure. The larger the weight average molecular weight of the fluoropolymer, the shorter the membrane microfibers, the larger the nodes, and the larger and fewer the holes. When the weight average molecular weight of the fluoropolymer meets this range, the porosity of the membrane can be increased while ensuring the length of the membrane microfibers.
[0029] Wherein, when the fluorine-containing polymer is polytetrafluoroethylene, the weight average molecular weight is preferably 3 million to 4 million g / mol; when the fluorine-containing polymer is polyvinylidene fluoride, the weight average molecular weight is preferably 700,000 to 800,000 g / mol.
[0030] According to the present invention, preferably, the weight average molecular weight of the polyethylene glycol is 4000-5000 g / mol. When the weight average molecular weight of the polyethylene glycol meets this range, it is difficult to form finger-like holes penetrating the fiber, and a more uniform finger-like hole structure is obtained.
[0031] According to the present invention, preferably, the pores of the fiber microporous membrane have a pore size of 10-500 μm, preferably 20-50 μm. When the pore size meets this range, particulate impurities with a particle size greater than 10 μm can be effectively controlled.
[0032] According to the present invention, preferably, the porosity of the fiber microporous membrane is 70-80%, preferably 75-80%;
[0033] According to the present invention, preferably, the specific surface area of the fiber microporous membrane is 300-1000m 2 / g, more preferably 900-1000m 2 / g.
[0034] According to the present invention, preferably, in step (1), the purity of the crude sulfur trioxide is greater than or equal to 99.5wt%, the particulate matter content contained in the crude sulfur trioxide is less than or equal to 400ppm, the iron content is less than or equal to 60ppm, and the sulfur dioxide content is less than or equal to 4000ppm.
[0035] In the present invention, ppm, ppb and ppt are unit symbols indicating solution concentration, wherein 1 ppm is 1 mg / L (milligram per liter), 1 ppb is 1 μg / L (microgram per liter), and 1 ppt is 1 ng / L (nanogram per liter).
[0036] According to the present invention, preferably, the content of sulfur dioxide in the semi-finished sulfuric acid solution is less than or equal to 1000 ppb. The content of sulfur dioxide in the semi-finished sulfuric acid solution is the same as the content of sulfur dioxide in the prepared electronic grade sulfuric acid.
[0037] According to the present invention, preferably, in step (3), the content of sulfuric acid in the electronic grade crude sulfuric acid is 96-98 wt % based on the total weight of the electronic grade crude sulfuric acid.
[0038] According to the present invention, the content of sulfuric acid contained in the electronic-grade crude sulfuric acid can be controlled by the concentration of the semi-finished sulfuric acid solution and the concentration temperature. The concentration adopts a concentration tower for evaporation concentration, and the concentration temperature is the bottom temperature of the concentration tower.
[0039] According to the present invention, preferably, based on the total weight of the semi-finished sulfuric acid solution, the content of sulfuric acid in the semi-finished sulfuric acid solution is 60-80 wt %.
[0040] According to the present invention, preferably, the concentration temperature is 130-150°C.
[0041] By controlling the concentration of the semi-finished sulfuric acid solution and the concentration temperature, not only the mass fraction of sulfuric acid in the electronic-grade sulfuric acid crude product can be controlled, but also the purity of the obtained electronic-grade sulfuric acid product can be further improved.
[0042] Furthermore, the concentration temperature is 130-140°C.
[0043] According to the present invention, preferably, the cooling temperature is 30-50°C.
[0044] In a preferred embodiment of the present invention, the content of sulfur dioxide contained in the electronic grade sulfuric acid is less than or equal to 1000 ppb, the content of particulate impurities contained in the electronic grade sulfuric acid is less than or equal to 50 pieces / mL, and the content of single metal cations contained in the electronic grade sulfuric acid is less than or equal to 100 ppt.
[0045] In a more preferred embodiment of the present invention, the content of sulfur dioxide contained in the electronic grade sulfuric acid is less than or equal to 500 ppb, the content of particulate impurities contained in the electronic grade sulfuric acid is less than or equal to 15 pieces / mL, and the content of single metal cations contained in the electronic grade sulfuric acid is less than or equal to 10 ppt.
[0046] In the present invention, ppb and ppt are both measured by mass.
[0047] The present invention will be described in detail below through examples and comparative examples. In the following examples and comparative examples, unless otherwise specified, all methods are conventional methods; and the reagents and materials used, unless otherwise specified, can be obtained from commercial sources.
[0048] The industrial sulfur trioxide raw material used in the following examples and comparative examples comes from Nanhua Company, with a purity greater than or equal to 99.5wt%. The particulate matter content in the industrial sulfur trioxide raw material is less than or equal to 400ppm, the iron content is less than or equal to 60ppm, and the sulfur dioxide content is less than or equal to 4000ppm.
[0049] Sulfur dioxide content was determined by potassium permanganate titration;
[0050] The content of particulate impurities was measured using a laser liquid particle counter;
[0051] The metal cation contents were determined using inductively coupled plasma mass spectrometry;
[0052] The non-metallic ion content was determined by turbidimetry and standard comparison method.
[0053] The following preparation examples are used to illustrate the preparation of fiber microporous membranes.
[0054] Preparation Example 1
[0055] The preparation method of the fiber microporous membrane is as follows:
[0056] Polytetrafluoroethylene (weight average molecular weight of 3 million g / mol) and polyethylene glycol (weight average molecular weight of 4000 g / mol) were fully mixed and granulated, and the obtained granules were passed through a twin-screw spinning machine and nitrogen was introduced. After the spinning was cooled and solidified, it was wound into a film, and then washed, dried and stretched. The amount of polyethylene glycol was 8wt% based on the weight of polytetrafluoroethylene. The pore size was 28μm, the porosity was 75%, and the specific surface area was 1000m 2 / g of fiber microporous membrane S1.
[0057] Preparation Example 2
[0058] A fiber microporous membrane was prepared according to the method of Preparation Example 1, except that polytetrafluoroethylene with a weight average molecular weight of 4 million g / mol and polyethylene glycol with a weight average molecular weight of 400 g / mol were selected, wherein the amount of polyethylene glycol was 6 wt % based on the weight of polytetrafluoroethylene. The obtained pore size was 400 μm, the porosity was 70%, and the specific surface area was 400 m 2 / g of fiber microporous membrane S2.
[0059] Preparation Example 3
[0060] The fiber microporous membrane was prepared according to the method of Preparation Example 1, except that polyvinylidene fluoride with a weight average molecular weight of 700,000 g / mol was selected. The obtained pore size was 10 μm, the porosity was 70%, and the specific surface area was 600 m 2 / g of fiber microporous membrane S3.
[0061] Preparation Example 4
[0062] The fiber microporous membrane was prepared according to the method of Preparation Example 1, except that polytetrafluoroethylene with a weight average molecular weight of 300,000 g / mol was selected. The pore size was 5 μm, the porosity was 50%, and the specific surface area was 500 m 2 / g of fiber microporous membrane S4.
[0063] Preparation Example 5
[0064] A fiber microporous membrane was prepared according to the method of Preparation Example 1, except that polyethylene glycol with a weight average molecular weight of 8000 g / mol was selected, and the amount of polyethylene glycol was 2 wt % based on the weight of polytetrafluoroethylene, resulting in a pore size of 40 μm, a porosity of 50%, and a specific surface area of 300 m 2 / g fiber microporous membrane S5.
[0065] Preparation Example 6
[0066] The fiber microporous membrane was prepared according to the method of Preparation Example 1, except that polysulfone with a weight average molecular weight of 70,000 g / mol was used. The obtained pore size was 70 μm, the porosity was 40%, and the specific surface area was 300 m 2 / g of fiber microporous membrane S6.
[0067] Preparation Example 7
[0068] The fiber microporous membrane was prepared according to the method of Preparation Example 1, except that polyethylene glycol was not added. The pore size was 30 μm, the porosity was 37%, and the specific surface area was 340 m 2 / g fiber microporous membrane S7.
[0069] Preparation Example 8
[0070] The preparation method of the polytetrafluoroethylene fiber membrane is as follows:
[0071] Polytetrafluoroethylene (weight average molecular weight of 3 million g / mol) and polyethylene glycol (weight average molecular weight of 4000 g / mol) are prepared into a blended polymer solution, which is made into fibers by electrospinning, and then washed and dried to obtain a polytetrafluoroethylene fiber membrane without a hollow structure.
[0072] Wherein, based on the weight of polytetrafluoroethylene, the amount of polyethylene glycol used is 8wt%.
[0073] The following example is used to illustrate the preparation of electronic grade sulfuric acid.
[0074] Example 1
[0075] In the ultra-clean production system, electronic grade sulfuric acid is prepared as follows:
[0076] (1) Vaporization: The industrial sulfur trioxide raw material is preheated and pumped into the evaporator to obtain gaseous sulfur trioxide raw material. The flow rate of the industrial sulfur trioxide raw material entering the evaporator is 40L / h, and the temperature of the evaporator is controlled at 120°C.
[0077] (2) Filtration and absorption using a fiber microporous membrane S1: The evaporated gaseous sulfur trioxide raw material and ultrapure water are passed through a fiber microporous membrane filter having a hollow structure for a residence time of 0.5 h to obtain a semi-finished sulfuric acid solution after the particulate impurities and sulfur dioxide are removed, so that the content of sulfuric acid in the semi-finished sulfuric acid solution is 80 wt % based on the total weight of the semi-finished sulfuric acid solution;
[0078] (3) Concentration: The semi-finished sulfuric acid solution obtained in step (2) is pumped into a concentration tower, and the tower bottom temperature is controlled to be 135° C. to obtain an electronic grade sulfuric acid crude product, wherein the content of sulfuric acid in the electronic grade sulfuric acid crude product is 96 wt % based on the total weight of the electronic grade sulfuric acid crude product.
[0079] (4) Cooling: The electronic grade sulfuric acid crude product obtained in step (3) is continuously cooled through two heat exchangers, and the temperature is controlled at 40° C. The by-product steam of the heat exchanger is used for preheating the raw material.
[0080] (5) Filtration: The cooled electronic-grade sulfuric acid crude product is filtered to obtain a high-purity electronic-grade sulfuric acid product that meets the standards and is stored in a sulfuric acid storage tank.
[0081] Example 2
[0082] Electronic grade sulfuric acid was prepared according to the method of Example 1, except that in step (2), a fiber microporous membrane S2 was used for filtration and absorption. A semi-finished sulfuric acid solution with a sulfuric acid content of 80 wt % was obtained, and then a crude electronic grade sulfuric acid with a sulfuric acid content of 96 wt % was obtained, and then a finished electronic grade sulfuric acid product was obtained.
[0083] Example 3
[0084] Electronic grade sulfuric acid was prepared according to the method of Example 1, except that the concentration and concentration temperature of the semi-finished sulfuric acid solution were different. Specifically, in step (2), the content of sulfuric acid in the semi-finished sulfuric acid solution was 70wt% based on the total weight of the semi-finished sulfuric acid solution; in step (3), the tower bottom temperature was controlled to be 150°C to obtain a crude electronic grade sulfuric acid product, so that the content of sulfuric acid in the crude electronic grade sulfuric acid product was 96wt% based on the total weight of the crude electronic grade sulfuric acid product. The finished electronic grade sulfuric acid product was obtained.
[0085] Embodiment 4-6
[0086] Electronic grade sulfuric acid was prepared according to the method of Example 1, except that different fiber microporous membranes were selected. Specifically, in step (2), fiber microporous membranes S3-S5 were used for filtration and absorption, respectively. A semi-finished sulfuric acid solution with a sulfuric acid content of 80 wt% was obtained, and then a crude electronic grade sulfuric acid with a sulfuric acid content of 96 wt% was obtained, and then a finished electronic grade sulfuric acid product was obtained.
[0087] Comparative Example 1
[0088] Electronic grade sulfuric acid was prepared according to the method of Example 1, except that in step (2), a fiber microporous membrane S6 was used for filtration and absorption. A semi-finished sulfuric acid solution with a sulfuric acid content of 81 wt% was obtained, and then a crude electronic grade sulfuric acid with a sulfuric acid content of 96 wt% was obtained, and then a finished electronic grade sulfuric acid product was obtained.
[0089] However, after 12 hours of operation, the sulfur dioxide content at the outlet of the fiber microporous membrane filter was 335 ppm, and the filter membrane was partially broken under the long-term impact of the acidic solution.
[0090] Comparative Example 2
[0091] Electronic grade sulfuric acid was prepared according to the method of Example 1, except that no fiber microporous membrane was used for filtration and absorption, and the gaseous sulfur trioxide raw material obtained in step (1) was directly reacted with ultrapure water for 0.5 h to obtain a semi-finished sulfuric acid solution with a sulfuric acid content of 80 wt %, and then to obtain a crude electronic grade sulfuric acid with a sulfuric acid content of 96 wt %, and then to obtain a finished electronic grade sulfuric acid product.
[0092] Comparative Example 3
[0093] Electronic grade sulfuric acid was prepared according to the method of Example 1, except that a fiber microporous membrane S7 without polyethylene glycol was used for filtration and absorption. A semi-finished sulfuric acid solution with a sulfuric acid content of 81 wt % was obtained, and then a crude electronic grade sulfuric acid with a sulfuric acid content of 96 wt % was obtained, and then a finished electronic grade sulfuric acid product was obtained.
[0094] Comparative Example 4
[0095] Electronic grade sulfuric acid was prepared according to the method of Example 1, except that in step (2), the polytetrafluoroethylene fiber membrane prepared in Preparation Example 8 was used for filtration and absorption. A semi-finished sulfuric acid solution with a sulfuric acid content of 80 wt % was obtained, and then a crude electronic grade sulfuric acid with a sulfuric acid content of 96 wt % was obtained, and then a finished electronic grade sulfuric acid product was obtained.
[0096] The sulfur dioxide content, particulate impurity content and ion content of the finished electronic-grade sulfuric acid obtained in each embodiment and comparative example were measured, and the measurement results are shown in Table 1. Wherein, Li to V all represent the metal element content.
[0097] Table 1
[0098]
[0099]
[0100] Table 1 (continued)
[0101]
[0102]
[0103] It can be seen from the results in Table 1 that high-purity electronic-grade sulfuric acid can be prepared by the preparation method provided by the present invention. The electronic-grade sulfuric acid prepared in Examples 1-6 has a sulfur dioxide content of less than or equal to 1000 ppb, a particulate impurity content of less than or equal to 50 particles / mL, and a single metal cation content of less than or equal to 100 ppt. In Comparative Example 1, polysulfone was used to prepare a fiber microporous membrane for filtration and absorption. Due to the poor chemical corrosion resistance, high temperature resistance and oxidation resistance of the prepared fiber microporous membrane, after 12 hours of operation, the filter membrane was partially broken under the long-term impact of the acidic solution, resulting in a significant increase in the sulfur dioxide content, particulate impurity content and ion content of the electronic-grade sulfuric acid product; in Comparative Example 3, a fiber microporous membrane without polyethylene glycol was used for filtration and absorption. The porosity of the prepared fiber microporous membrane was significantly reduced, resulting in a significant increase in the sulfur dioxide content, particulate impurity content and ion content of the electronic-grade sulfuric acid product; in Comparative Example 2, a fiber microporous membrane was not used for filtration and absorption. In Comparative Example 4, a polytetrafluoroethylene fiber membrane without a hollow structure was used for filtration and absorption. Compared with Examples 1-6, the sulfur dioxide content, particulate impurity content and ion content of the electronic-grade sulfuric acid product were significantly improved, and the purity was greatly reduced.
[0104] In addition, Example 2 uses polyethylene glycol with a lower weight-average molecular weight. Compared with Example 1, the pore size of the obtained fiber microporous membrane is increased, and the porosity and specific surface area are reduced, resulting in an increase in the sulfur dioxide content, particulate impurity content and partial ion content of the electronic-grade sulfuric acid product; Example 3 changes the concentration and concentration temperature of the semi-finished sulfuric acid solution. Compared with Example 1, the sulfur dioxide content, particulate impurity content and partial ion content of the obtained electronic-grade sulfuric acid product are increased, indicating that controlling the concentration of the semi-finished sulfuric acid solution and the concentration temperature have a greater influence on the purity of the obtained electronic-grade sulfuric acid product; Example 4 uses polyvinylidene fluoride to prepare a fiber microporous membrane, and the obtained fiber The mechanical strength of the microporous membrane is weakened, and the pore size, porosity and specific surface area are reduced, thereby increasing the sulfur dioxide content, particulate impurity content and ion content of the electronic grade sulfuric acid product obtained; Example 5 uses polytetrafluoroethylene with a smaller weight average molecular weight, and the obtained fiber microporous membrane has a reduced pore size, reduced porosity and specific surface area, resulting in an increase in the sulfur dioxide content, particulate impurity content and ion content of the electronic grade sulfuric acid product; Example 6 uses polyethylene glycol with a larger weight average molecular weight and reduces its addition amount, and the porosity and specific surface area of the obtained fiber microporous membrane are reduced, resulting in an increase in the sulfur dioxide content, particulate impurity content and ion content of the electronic grade sulfuric acid product obtained. This shows that by selecting the appropriate type of fluorinated polymer, the weight average molecular weight of polyethylene glycol and polytetrafluoroethylene, and the addition amount of polyethylene glycol, a fiber microporous membrane with moderate pore size, porosity and specific surface area and high mechanical strength can be obtained, thereby improving the purity of the electronic grade sulfuric acid product. In addition, by selecting the appropriate concentration and concentration temperature of the semi-finished sulfuric acid solution, the purity of the electronic grade sulfuric acid product is further improved.
[0105] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing electronic grade sulfuric acid, It is characterized in that The preparation method comprises the following steps: (1) vaporizing crude sulfur trioxide to obtain a gaseous sulfur trioxide raw material; (2) filtering and absorbing the gaseous sulfur trioxide raw material and ultrapure water through a fiber microporous membrane to obtain a semi-finished sulfuric acid solution; (3) concentrating the semi-finished sulfuric acid solution to obtain an electronic grade sulfuric acid crude product; (4) cooling and filtering the crude electronic-grade sulfuric acid to obtain the electronic-grade sulfuric acid; The fiber microporous membrane is prepared by granulating, spinning, winding and stretching a mixture of fluorine-containing polymer and polyethylene glycol.
2. The preparation method according to claim 1, It is characterized in that In the mixture, the amount of the polyethylene glycol is 6-10 wt % based on the weight of the fluorine-containing polymer; Preferably, the fluorine-containing polymer is at least one selected from polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride, fluorinated ethylene-propylene copolymer, ethylene-tetrafluoroethylene copolymer and chlorotrifluoroethylene-ethylene copolymer, preferably polytetrafluoroethylene; Preferably, the weight average molecular weight of the fluorine-containing polymer is 300,000-4,000,000 g / mol; Preferably, the weight average molecular weight of the polyethylene glycol is 4000-5000 g / mol.
3. The preparation method according to claim 1 or 2, It is characterized in that The pores of the fiber microporous membrane have a pore size of 10-500 μm, preferably 20-50 μm; Preferably, the porosity of the fiber microporous membrane is 70-80%, preferably 75-80%; Preferably, the specific surface area of the fiber microporous membrane is 300-1000m 2 / g, preferably 900-1000m 2 / g.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that In step (1), the purity of the crude sulfur trioxide is greater than or equal to 99.5wt%, the particulate matter content contained in the crude sulfur trioxide is less than or equal to 400ppm, the iron content is less than or equal to 60ppm, and the sulfur dioxide content is less than or equal to 4000ppm.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The content of sulfur dioxide contained in the semi-finished sulfuric acid solution is less than or equal to 1000 ppb.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that In step (3), based on the total weight of the crude electronic-grade sulfuric acid, the content of sulfuric acid in the crude electronic-grade sulfuric acid is 96-98 wt %.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that Based on the total weight of the semi-finished sulfuric acid solution, the content of sulfuric acid in the semi-finished sulfuric acid solution is 60-80wt%.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that The concentration temperature is 130-150°C, preferably 130-140°C.
9. The preparation method according to any one of claims 1 to 8, It is characterized in that The cooling temperature is 30-50°C.
10. The preparation method according to any one of claims 1 to 9, It is characterized in that The content of sulfur dioxide contained in the electronic grade sulfuric acid is less than or equal to 1000 ppb, the content of particulate impurities contained in the electronic grade sulfuric acid is less than or equal to 50 pieces / mL, and the content of single metal cations contained in the electronic grade sulfuric acid is less than or equal to 100 ppt; Preferably, the content of sulfur dioxide in the electronic-grade sulfuric acid is less than or equal to 500 ppb, the content of particulate impurities in the electronic-grade sulfuric acid is less than or equal to 15 pieces / mL, and the content of single metal cations in the electronic-grade sulfuric acid is less than or equal to 10 ppt.
Citation Information
Patent Citations
Melt-spinning preparation method of polyvinylidene fluoride hollow fiber filter membrane
CN108977903A
Method for preparing ultra-pure sulfuric acid by a combined membrane method
CN109485022A
Process for removing low-boiling-point organic matters in high-concentration wastewater
CN114538685A
Marine tail gas desulfurization device based on membrane absorption technology
CN216630283U