Self-assembled spherical boron nitride and preparation method thereof

By self-assembling spherical boron nitride on the growth substrate and using sheet boron nitride to form a 0-dimensional-2-dimensional hierarchical structure, the problems of carbon removal and high-temperature operation in the prior art are solved, and high-purity spherical boron nitride is achieved The simple and efficient preparation of the company has expanded its application in the field of functional composite materials.

CN118929587AActive Publication Date: 2024-11-12LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +1

Patent Information

Application Number
CN202411180876.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The prior art requires carbon removal treatment when preparing spherical boron nitride. The process is cumbersome and the high-temperature operation requires high equipment requirements, making it difficult to achieve efficient and simple preparation of high-purity spherical boron nitride.

Method used

By thoroughly grinding and mixing the silicon dioxide and boron powder, place it under a growth substrate to heat up in an inert gas stream and switch to ammonia for ammonia treatment, forming a self-assembled spherical boron nitride, and self-assembly using sheet boron nitride to form 0 Dimension-2-dimensional hierarchical structure avoids carbon removal and high temperature operations.

Benefits of technology

It achieves a simple process and no need to remove impurities to obtain high-purity spherical boron nitride, providing a simple and efficient preparation method, broadening the application prospects of boron nitride in the field of functional composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929587A_ABST
    Figure CN118929587A_ABST
Patent Text Reader

Abstract

The invention discloses self-assembled spherical boron nitride and a preparation method thereof, and the method comprises the following steps: fully grinding and mixing silicon dioxide and boron powder to obtain a boron-containing precursor; and placing the obtained boron-containing precursor below a growth substrate, heating to 1400-1500 DEG C in inert gas flow, switching the inert gas flow into ammonia gas, carrying out ammonification treatment at 1400-1500 DEG C, switching the ammonia gas into inert gas flow, cooling to room temperature, and loading white self-assembled spherical boron nitride on the surface of the growth substrate. The problems that in the prior art, carbon removal treatment needs to be conducted on a product, the working procedure process is tedious, and the requirement for equipment by high-temperature operation is high are solved, the spherical boron nitride is formed by self-assembling boron nitride of a sheet structure into a sphere, and a 0-dimensional to 2-dimensional hierarchical structure is formed; and respective advantages and multi-dimensional synergistic effects of the sheet-shaped and spherical structures can be fully exerted. The process is simple, and the high-purity spherical boron nitride can be obtained without removing impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing boron nitride, in particular to self-assembled spherical boron nitride and a method for preparing the same. Background Art

[0002] Hexagonal boron nitride (h-BN) has low density, large specific surface area, high mechanical strength and excellent thermal properties, especially compared with metal fillers and carbon-based nanomaterials, boron nitride has excellent electrical insulation properties. Because it can significantly improve the mechanical and thermal properties of polymers without changing their electrical properties, it has been widely used in electronics / optoelectronics, catalysis, energy storage and conversion, sensor and electronic product development, nanocomposites and other fields.

[0003] Boron nitride has a series of structures, such as zero-dimensional spheres, one-dimensional tubes, rods, and two-dimensional sheets. Among the different structures, spherical BN has received special attention due to its isotropy. h-BN is a typical layered material, and crystal growth tends to grow laterally along the (002) plane rather than along the thickness direction. Therefore, it is difficult for h-BN to grow in an arch shape and form isotropic spherical particles. Compared with the preparation of rods, tubes, and sheets, there are fewer reports on the synthesis of spherical boron nitride, and most studies use toxic reactants, expensive equipment, or complex synthesis conditions.

[0004] The prior art for preparing spherical boron nitride usually requires the introduction of carbon-containing materials for carbon thermal reduction at high temperature, and in order to obtain a high-purity product, the product must ultimately be decarbonized. The process is cumbersome and requires high equipment requirements to be operated at high temperatures. Summary of the invention

[0005] The purpose of the present invention is to provide a self-assembled spherical boron nitride and a preparation method thereof, which solves the problems in the prior art that the product needs to be decarbonized, the process is cumbersome, and the high-temperature operation requires high equipment requirements. The three-dimensional spherical boron nitride formed by the self-assembly of flake boron nitride has a 0-dimensional-2-dimensional hierarchical structure, which can give full play to the respective advantages of the flake and spherical structures and the multi-dimensional synergistic effect.

[0006] In order to achieve the above object, the present invention provides a method for preparing self-assembled spherical boron nitride, the method comprising:

[0007] (1) grinding and mixing silicon dioxide and boron powder to obtain a boron-containing precursor;

[0008] (2) placing the obtained boron-containing precursor under a growth substrate, heating it to 1400°C to 1500°C in an inert gas flow, switching the inert gas flow to ammonia gas, and performing an ammoniation treatment at 1400°C to 1500°C. After the reaction is completed, switching the ammonia gas to an inert gas flow and cooling it to room temperature, white self-assembled spherical boron nitride is loaded on the surface of the growth substrate, and the molar ratio of the silicon dioxide to the boron powder is 1:(5-20).

[0009] The main influencing factors of this method include: ammoniation temperature and the ratio of silicon dioxide to boron powder. The reaction degree of the boron source is different at different ammoniation temperatures. 1400℃~1500℃ is conducive to the reaction of the boron source, promoting the reaction degree and improving the purity of the product. If the temperature is too high, the growth substrate cannot withstand such a high temperature, so that the product cannot be deposited on the growth substrate to form the desired product. The molar ratio of silicon dioxide to boron powder is 1:(5~20). Boron powder can provide more active substances at the ammoniation temperature, so that the self-assembled spherical boron nitride can load larger flake boron nitride. When the ratio of boron powder is too high, silicon dioxide and boron powder cannot generate enough active boron source to react with ammonia at high temperature; similarly, when there is too much silicon dioxide, it cannot generate enough active boron source to react with ammonia, and self-assembled spherical boron nitride with a 0-dimensional-2-dimensional hierarchical structure cannot be generated.

[0010] Preferably, the molar ratio of silicon dioxide to boron powder is 1:(10-20). Preferably, the growth substrate is a high-purity aluminum oxide sheet or a SiO2 / Si sheet.

[0011] Preferably, the inert gas flow is nitrogen, argon, helium, neon or radon, and its flow rate is 100 sccm.

[0012] Preferably, the heating rate is 1-15°C / min.

[0013] Preferably, the flow rate of the ammonia gas is 100 sccm.

[0014] Preferably, the ammoniation treatment lasts for 1 to 10 hours.

[0015] The invention provides a self-assembled spherical boron nitride prepared by the preparation method.

[0016] Preferably, the particle size of the self-assembled spherical boron nitride is 2 μm.

[0017] Preferably, the surface of the self-assembled spherical boron nitride is uniformly loaded with boron nitride with a flake structure.

[0018] The self-assembled spherical boron nitride and the preparation method thereof of the present invention solve the problems that the product needs to be decarbonized in the prior art, the process is cumbersome, and the high-temperature operation requires high equipment requirements, and has the following advantages:

[0019] 1. The spherical boron nitride of the present invention is self-assembled into a spherical shape by boron nitride with a flake structure, forming a 0-dimensional-2-dimensional hierarchical structure, which can give full play to the respective advantages of the flake and spherical structures and the multi-dimensional synergistic effect.

[0020] 2. The process of the present invention is simple, and high-purity spherical boron nitride can be obtained without impurity removal. It provides a simple and efficient method for synthesizing spherical boron nitride without the use of toxic reactants, improves the performance of the material and broadens the application of boron nitride materials in the field of functional composite materials. It has important application prospects in the field of functional composite materials and provides a basis for the large-scale preparation of high-quality and high-purity spherical boron nitride. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a 3.00kx SEM image of the sample prepared in Example 1 of the present invention.

[0022] Figure 2 This is a 20.0kx SEM image of the sample prepared in Example 1 of the present invention.

[0023] Figure 3 This is the X-ray diffraction (XRD) pattern of the sample prepared in Example 1 of the present invention.

[0024] Figure 4 This is the Fourier transform infrared (FTIR) spectrum of the sample prepared in Example 1 of the present invention.

[0025] Figure 5 This is a 10.0kx SEM image of a sample prepared in Example 2 of the present invention.

[0026] Figure 6 This is a 5.00kx SEM image of a sample prepared in Example 3 of the present invention.

[0027] Figure 7 5.00kx SEM image of the sample prepared for Comparative Example 1 of the present invention.

[0028] Figure 8 The 3.00kx SEM image of the sample prepared for Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] A method for preparing self-assembled spherical boron nitride, the method comprising:

[0032] (1) preparing a boron-containing precursor: grinding and mixing silicon dioxide and boron powder in a molar ratio of 1:10 to obtain a boron-containing precursor;

[0033] (2) Ammoniating treatment: The obtained boron-containing precursor is placed in an alumina crucible, and a high-purity alumina sheet is placed in the alumina crucible. After continuously heating to 1400°C at a heating rate of 2°C / min in a nitrogen atmosphere with a flow rate of 100sccm, the nitrogen is switched to 100sccm ammonia and the ammoniating treatment is carried out at 1400°C for 1h. After the reaction is completed, the ammonia is switched to 100sccm nitrogen. After cooling to room temperature, the high-purity alumina sheet is taken out. The surface of the high-purity alumina sheet is covered with white substance, which is self-assembled spherical boron nitride.

[0034] Example 2

[0035] A method for preparing self-assembled spherical boron nitride is substantially the same as that in Example 1, except that:

[0036] In step (1), the molar ratio of silicon dioxide to boron powder is adjusted from 1:10 to 1:5.

[0037] Example 3

[0038] A method for preparing self-assembled spherical boron nitride is substantially the same as that in Example 1, except that:

[0039] In step (1), the molar ratio of silicon dioxide to boron powder is adjusted from 1:10 to 1:20; in step (2), the ammoniation time is adjusted from 1400°C to 1500°C.

[0040] Comparative Example 1

[0041] A method for preparing self-assembled spherical boron nitride is substantially the same as that in Example 1, except that:

[0042] In step (2), the ammoniation temperature is changed to 1300° C., and the other steps are the same as those in Example 1, thereby obtaining a self-assembled spherical boron nitride-supported flake boron nitride structure.

[0043] Comparative Example 2

[0044] A method for preparing self-assembled spherical boron nitride is substantially the same as that in Example 2, except that:

[0045] In step (2), the amination temperature is changed to 1300° C., and the other steps are the same as those in Example 2, thereby obtaining a self-assembled spherical boron nitride-supported flake boron nitride structure.

[0046] Example 1 Characterization of Self-assembled Spherical Boron Nitride

[0047] The self-assembled spherical boron nitride prepared in Examples 1 and 2 and the products prepared in Comparative Examples 1 and 2 were observed using a scanning electron microscope, and X-ray diffraction and Fourier transform infrared analysis were performed.

[0048] like Figure 1 As shown in FIG. 3, the SEM image of the sample prepared in Example 1 of the present invention at 3.00kx. Figure 1 It can be seen that in Example 1, a large amount of spherical boron nitride is generated.

[0049] like Figure 2 As shown in FIG. 2 , the 20.0kx SEM image of the sample prepared in Example 1 of the present invention. Figure 2 It can be seen that the surface of the spherical boron nitride in Example 1 simultaneously carries boron nitride with a flake structure.

[0050] like Figure 3 As shown, the X-ray diffraction (XRD) spectrum of the sample prepared in Example 1 of the present invention, wherein the abscissa is 2θ and the ordinate is intensity. Figure 3 It can be seen that the peaks at 26.6°, 41.8°, 54.1° and 76.1° belong to the diffraction of hexagonal BN (JCPDS card number 34-0421), plane (002), (100), (004) and (110), respectively. The appearance of the sharp main peak (002) and the peak related to the (110) plane order indicates that the synthesized spherical BN crystallization is relatively good.

[0051] like Figure 4 As shown, the Fourier transform infrared (FTIR) spectrum of the sample prepared in Example 1 of the present invention, wherein the horizontal axis is the wave number and the vertical axis is the transmittance. Figure 4 It can be seen that the FTIR spectrum of spherical BN has two -1 and 1375cm -1 The sharp peaks of are due to the out-of-plane bending vibration of the BNB bond and the in-plane stretching vibration mode of the BN bond. -1 The peaks appearing nearby can be attributed to the OH bonds, proving the existence of -OH groups.

[0052] like Figure 5 As shown in the figure, the 10.0kx SEM image of the sample prepared in Example 2 of the present invention. Figure 5 It can be seen that a large amount of spherical boron nitride is generated in Example 2. Compared with Example 1, the difference of Example 2 is mainly that a smaller proportion of boron source is added, and the size of the flake boron nitride loaded on the self-assembled spherical boron nitride is smaller.

[0053] like Figure 6 As shown in the figure, the 5.00kx SEM image of the sample prepared in Example 3 of the present invention. Figure 6It can be seen that a large amount of spherical boron nitride is generated in Example 3. Compared with Example 1, the difference of Example 3 mainly lies in the addition of a larger proportion of boron source and a higher amination temperature, which further increases the size of the flake boron nitride loaded on the self-assembled spherical boron nitride.

[0054] like Figure 7 As shown, the 5.00kx SEM image of the sample prepared in Comparative Example 1 of the present invention. Figure 6 It can be seen that in Comparative Example 1, spherical boron nitride is generated, but impurities are generated.

[0055] like Figure 8 As shown, the 3.00kx SEM image of the sample prepared in Comparative Example 2 of the present invention. Figure 7 It can be seen that in Comparative Example 2, spherical boron nitride is generated, but a large amount of impurities are generated.

[0056] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing self-assembled spherical boron nitride, characterized in that: The method includes: (1) grinding and mixing silicon dioxide and boron powder to obtain a boron-containing precursor; (2) placing the obtained boron-containing precursor under a growth substrate, heating it to 1400° C. to 1500° C. in an inert gas flow, switching the inert gas flow to ammonia gas, and performing an ammoniation treatment at 1400° C. to 1500° C. After the reaction is completed, switching the ammonia gas to an inert gas flow and cooling it to room temperature, a white self-assembled spherical boron nitride is loaded on the surface of the growth substrate; The molar ratio of the silicon dioxide to the boron powder is 1:(5-20).

2. The preparation method according to claim 1, characterized in that: The molar ratio of the silicon dioxide to the boron powder is 1:(10-20).

3. The preparation method according to claim 1, characterized in that: The growth substrate is a high-purity aluminum oxide sheet or a SiO2 / Si sheet.

4. The preparation method according to claim 1, characterized in that: The inert gas flow is nitrogen, argon, helium, neon or radon, and its flow rate is 100 sccm.

5. The preparation method according to claim 1, characterized in that: The heating rate is 1-15°C / min.

6. The preparation method according to claim 1, characterized in that: The flow rate of the ammonia gas is 100 sccm.

7. The preparation method according to claim 1, characterized in that: The time of the ammoniation treatment is 1 to 10 hours.

8. A self-assembled spherical boron nitride obtained by the preparation method according to any one of claims 1 to 7.

9. The self-assembled spherical boron nitride according to claim 8, characterized in that: The particle size of the self-assembled spherical boron nitride is 2 μm.

10. The self-assembled spherical boron nitride according to claim 8, characterized in that: The surface of the self-assembled spherical boron nitride is uniformly loaded with boron nitride with a flake structure.

Citation Information

Patent Citations

  • Boron nitride agglomerates, method for the production thereof and usage thereof

    CN104284860A

  • Method for synthesizing spherical boron nitride (BN) nano-powder under induction of amorphous precursor

    CN110386593A

  • Method for producing spherical boron carbide powder

    JP2020142971A

  • Direct formation of hexagonal boron nitride on silicon based dielectrics

    US20190097000A1

Cited By

  • Preparation method of spherical boron nitride

    CN120117577A