Method for recycling waste sodium ion precursor resource

Through multiple washing and acid dissolving of sodium ion battery precursors, combined with copper and nickel extraction processes, selectively removing heavy metal elements, the waste treatment problem in the production of sodium ion battery precursors is solved, and the efficient resource regeneration is achieved Improve utilization and economicality.

CN118929607APending Publication Date: 2024-11-12浙江格派钴业新材料有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410994702.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the production process of sodium ion battery precursors, the treatment of waste precursors is difficult, resulting in large water consumption, poor effect, high unit consumption, and inability to effectively utilize heavy metal ions, resulting in waste of resources.

Method used

Cu, Ni, Fe or Mn elements are selectively removed by multiple washing and acid dissolving, and these elements are extracted through copper and nickel extraction processes, and then reacted with precipitant to prepare synthetic materials to achieve resource reuse .

Benefits of technology

It increases the added value of waste in the production process of precursors, simplifies the wastewater treatment process, reduces operating costs, and flexibly selects the removal method of heavy metal elements according to different sources, improving economic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929607A_ABST
    Figure CN118929607A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of new energy material preparation, and particularly relates to a waste sodium ion precursor resource recycling method. The invention aims to solve the problem that heavy metal ions in a waste precursor generated in the production process of a sodium electric precursor are fully utilized, and provides a method for recycling a waste sodium ion precursor resource, so that the additional value of wastes in the production process of the precursor is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new energy material preparation, and in particular relates to a method for recycling waste sodium ion precursor resources. Background Art

[0002] In the new energy vehicle and energy storage industries, sodium-ion batteries have ushered in their own highlight moments under the background of the rapid advancement of sodium battery research and development in the industry. The research and development strategy of layered oxide positive electrodes for sodium-ion batteries is similar to that of lithium battery ternary materials. They are the first to be mass-produced due to their mature technology, high energy density, low cost, and equipment compatibility. Its precursor can also be prepared according to a similar ternary precursor process. Generally, nickel salts (copper salts), iron salts, and manganese salts are mixed in a certain proportion; sodium hydroxide and ammonia water are mixed; the ammonia-alkali solution and the metal mixed solution are fully reacted to generate a co-precipitation product; the co-precipitation product is filtered and washed, and heated and dried to obtain a layered oxide precursor.

[0003] In the process of precursor preparation, due to the small solubility product of nickel salt (copper salt), iron salt and manganese salt hydroxide, the fast precipitation rate, high solution supersaturation, fast crystal nucleation, easy formation of colloidal precipitation, and the difficult control of morphology, it is inevitable to produce a large amount of waste precursors due to the influence of various factors such as the supersaturation of precipitated ions in the reaction system, pH value, ammonia concentration, temperature, stirring, rate, etc. Most factories discharge it together with the precursor washing wastewater, resulting in the disadvantages of large water consumption, poor effect, high unit consumption and high operating cost for the recycling and treatment of precursor washing wastewater. Although many environmental design companies have developed zero-discharge process technology for precursor wastewater, the process treatment scheme is single, and the actual situation of each enterprise is different, and there are many problems in the actual operation process.

[0004] With the rapid development of the new energy vehicle industry, the installed capacity of sodium-ion batteries in the upstream of its industrial chain has increased significantly, and the wastewater generated is also a problem we have to face. In order to fundamentally solve the "concentration discharge" problem, it is of great significance to provide a method for recycling waste sodium-ion precursor resources. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of waste precursors generated in the production process of sodium electric precursors, make full use of the heavy metal ions therein, provide a method for recycling waste sodium ion precursor resources, and effectively increase the added value of waste in the precursor production process. The specific scheme is as follows:

[0006] A method for recycling waste sodium ion precursor resources comprises the following steps:

[0007] S1: washing and removing impurities from the waste precursors generated during the synthesis of sodium electrode precursors for multiple times;

[0008] S2: Add water and reducing agent into the dissolution tank, start stirring, put in the waste precursor, and slowly add acid into the reaction system to dissolve;

[0009] S3: selectively removing the Cu, Ni, Fe or Mn elements in the above solution as needed and using them as raw materials for subsequent synthetic materials;

[0010] The removal of Cu adopts a copper extraction process, and the Cu ion extractant is prepared by mixing one, two or three of aldoxime, ketoxime and a modifier with a diluent. The specific steps of the copper extraction process are as follows: preparing a copper extractant with a volume concentration of 10% to 20%; the functional sections of the extraction tank are distributed as follows: 4 extraction sections, 2 washing sections, and 4 stripping sections; during the copper extraction process, the ratio of the organic phase to the aqueous phase is between 1:3 and 1:8, the temperature of the extraction system is 40 to 50°C, and the copper content of the solution after the copper extraction is controlled to be below 0.0005g / L;

[0011] The removal of Ni adopts a nickel extraction process, and the Ni ion extractant is selected from phosphine extractants Mextral204P, Mextral507P, Cyanex272, Cyanex301 or Cyanex302; amine extractants Alamine336 or Alquit33; hydroxime extractants Mextral63H, Mextral84H, Mextral984H or Mextral860H; carboxylic acid and carboxylic acid pyridine ester extractants Ver satic10, CLX50 or 4PC, the specific steps of the nickel extraction process are as follows: prepare an extractant with a volume concentration of 30% to 40%; the functional sections of the extraction tank are distributed as follows: 12 extraction sections, 10 washing sections, and 8 stripping sections; use a 32% liquid alkali solution to saponify the organic phase, and the saponification rate is controlled at 50% to 60%; during the nickel extraction process, the organic phase to water phase ratio is between 3:1 and 5:1, the extraction temperature is between 40 and 50°C, and nickel is extracted, and the nickel content of the solution after nickel extraction is controlled to be below 0.0005g / L;

[0012] S4: After the impurity-removed solution is concentrated, it is reacted with a precipitant, and then solid-liquid separation is performed (after extraction, nickel manganese hydroxide / carbonate (for synthesizing lithium nickel manganese oxide), iron manganese phosphate / oxalate (for synthesizing lithium iron manganese phosphate) can be prepared by coprecipitation reaction, and lithium iron manganese phosphate can be prepared by hydrothermal synthesis reaction);

[0013] The chemical formula of the waste sodium ion precursor is Ni a Cu b Fe c Mn d (OH) 2 , a+b+c+d=1;

[0014] The washing in S1 is performed by multiple washing with hot pure water at 30-70° C. until the conductivity is ≤200 us / cm.

[0015] 0.05-2% of reducing agent is added according to the mass of the precursor.

[0016] The reducing agent includes one of hydrazine hydrate, ascorbic acid, pyrosulfite and sulfur dioxide.

[0017] The acid in S2 is one or a mixture of sulfuric acid, nitric acid, phosphoric acid, hydrochloric acid, perchloric acid, hydrobromic acid, hydroiodic acid, citric acid, oxalic acid, formic acid, etc. When sulfuric acid is used to dissolve the precursor, the following reaction occurs:

[0018] Ni a Cu b Fe c Mn d (OH) 2 +SO 4 2- +2H + →aCuSO4+bNiSO4+cMnSO4+dFeSO4+2H2O.

[0019] The temperature of the reaction system in S2 is 30-60° C., the pH is 2-5, and the solid-liquid ratio in the reaction tank is controlled between 1:3 and 1:5.

[0020] The Cu ion extractant is N902 copper extractant, and the Ni ion extractant is Cyanex272 extractant. In the precursor production process, due to inaccurate control, a large amount of waste precursors are discharged into the wastewater, resulting in the wastewater containing not only a large amount of ammonia nitrogen, sulfate ions, and sodium ions, but also a large amount of heavy metal elements, resulting in a large amount of water consumption, poor effect, high unit consumption, and high operating costs for wastewater recycling and treatment; and the waste precursors themselves are mostly high-purity Cu, Ni, Fe, Mn hydroxides and a small amount of soluble sulfate ions, sodium ions, and ammonia nitrogen. Therefore, the waste precursors can be directly recycled and reused, turning waste into treasure, and at the same time reducing the difficulty of wastewater treatment.

[0021] The present invention provides such a method for recycling waste sodium ion precursor resources, and the advantages of this technical solution are as follows:

[0022] 1) Compared with the recycling and reuse of precursor wastewater, the waste precursor has higher purity, the treatment process is relatively simple, and there is no need for a multi-step impurity removal process;

[0023] 2) Solve the problem of waste precursors from the root, avoid discharge with wastewater, and increase the difficulty of wastewater treatment;

[0024] 3) According to the different sources of waste precursors, heavy metal elements can be flexibly and selectively removed, so that the obtained solution can be directly used to prepare different precursors, which is more economical. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic flow chart of a method for recycling waste sodium ion precursor resources according to the present invention;

[0026] Figure 2 It is the SEM image of the waste sodium ion precursor;

[0027] Figure 3 This is a SEM image of the ferrous manganese oxalate precursor prepared in Example 1;

[0028] Figure 4 This is the XRD pattern of the iron manganese phosphate precursor prepared in Example 2;

[0029] Figure 5 This is the SEM image of the hydrothermal lithium iron manganese phosphate precursor prepared in Example 3. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0031] Production process such as Figure 1 As shown, the specific steps are as follows:

[0032] Example 1

[0033] The iron manganese oxalate precursor was prepared by coprecipitation reaction.

[0034] S1: The waste precursor Ni 0.2 Fe 0.4 Mn 0.4 Use 50℃ hot water for washing, and stop washing when the conductivity of washing water is 150us / cm measured by conductivity meter;

[0035] S2: Add 4.5 kg of deionized water and 15 g of ascorbic acid to the acidic dissolution tank, stir at 300 rpm, and add 1.5 kg of the waste precursor Ni 0.2 Fe 0.4 Mn 0.4 , slowly add sulfuric acid, adjust the pH to 3.0, and control the temperature of the reaction system at 40°C until the waste precursor is completely dissolved.

[0036] S3: nickel extraction, specifically as follows: prepare Cyanex272 extractant with a volume concentration of 35%; set the distribution of each functional section of the extraction tank: 12 extraction sections, 10 washing sections, and 8 stripping sections, use 32% liquid alkali solution to saponify the organic phase, and the saponification rate is controlled at 55%; the ratio of organic to aqueous phase is 3:1, the extraction temperature is 40°C, and nickel is extracted. After nickel extraction, the nickel content of the solution is 0.0003g / L.

[0037] S4: Concentrate the FeMn metal ions in the solution to 2 mol / L and add Na 2 C 2 O 4 ·H 2 O and H 2 C 2 O 4 ·2H 2 O (50:1), a light yellow precipitate was formed, and the FeMn metal ions in the solution were concentrated to 2 mol / L and dried at 65 °C under vacuum to obtain the precursor powder Mn 0.5 Fe 0.5 C 2 O 4 ·2H 2 O.

[0038] Example 2

[0039] The iron-manganese phosphate precursor was prepared by coprecipitation reaction.

[0040] S1: The waste precursor Ni 0.2 Fe 0.4 Mn 0.4 Use 50℃ hot water for washing, and stop washing when the conductivity of washing water is 150us / cm measured by conductivity meter;

[0041] S2: Add 4.5 kg of deionized water and 15 g of ascorbic acid to the acidic dissolution tank, stir at 300 rpm, and add 1.5 kg of the waste precursor Ni 0.2 Fe 0.4 Mn 0.4 , slowly add sulfuric acid, adjust the pH to 3.0, and control the temperature of the reaction system at 40°C until the waste precursor is completely dissolved.

[0042] S3: nickel extraction, specifically as follows: prepare Cyanex272 extractant with a volume concentration of 35%; set the distribution of each functional section of the extraction tank: 12 extraction sections, 10 washing sections, and 8 stripping sections, use 32% liquid alkali solution to saponify the organic phase, and the saponification rate is controlled at 55%; the ratio of organic to aqueous phase is 3:1, the extraction temperature is 40°C, and nickel is extracted. After nickel extraction, the nickel content of the solution is 0.0003g / L.

[0043] S4: The FeMn metal ions in the solution are concentrated to 2 mol / L, and added to the reactor with phosphoric acid, sodium hexadecyl sulfate, and hydrogen peroxide. The pH value of the system is controlled at 3-3.5, the temperature of the reactor solution is 70°C, and the reaction is stirred at 130 rpm for 5 hours to obtain a suspension. The suspension is filtered and washed with a filter press to obtain, and then calcined at 380°C to remove free water and crystal water to obtain iron manganese phosphate precursor Mn 0.5 Fe 0.5 PO 4 .

[0044] Example 3

[0045] Lithium iron manganese phosphate was prepared by hydrothermal reaction.

[0046] S1: The waste precursor Ni 0.2 Fe 0.4 Mn 0.4 Use 50℃ hot water for washing, and stop washing when the conductivity of washing water is 150us / cm measured by conductivity meter;

[0047] S2: Add 4.5 kg of deionized water and 15 g of ascorbic acid to the acidic dissolution tank, stir at 300 rpm, and add 1.5 kg of the waste precursor Ni 0.2 Fe 0.4 Mn 0.4 , slowly add sulfuric acid, adjust the pH to 3.0, and control the temperature of the reaction system at 40°C until the waste precursor is completely dissolved.

[0048] S3: nickel extraction, specifically as follows: prepare Cyanex272 extractant with a volume concentration of 35%; set the distribution of each functional section of the extraction tank: 12 extraction sections, 10 washing sections, and 8 stripping sections, use 32% liquid alkali solution to saponify the organic phase, and the saponification rate is controlled at 55%; the ratio of organic to aqueous phase is 3:1, the extraction temperature is 40°C, and nickel is extracted. After nickel extraction, the nickel content of the solution is 0.0003g / L.

[0049] S4: The FeMn metal ions in the solution were concentrated to 2 mol / L, phosphoric acid and lithium hydroxide were dissolved in a mixed solvent consisting of water and ethylene glycol in a volume ratio of 1:2 according to Li:(Fe+Mn):P=3.03:1:P, and the solution was placed in a high-temperature and high-pressure reactor. The volume of the solution was 80% of the volume of the reactor. The solution was heated to 240°C and the reaction time was 6 hours. After natural cooling, the solution was centrifuged and washed three times, and then vacuum dried to obtain lithium iron manganese phosphate (LiFe 0.5 Mn 0.5 PO 4 )front drive.

[0050] Example 4

[0051] The iron manganese oxalate precursor was prepared by coprecipitation reaction.

[0052] S1: The waste precursor Cu 0.5 Fe 0.2 Mn 0.3 Use 50℃ hot water for washing, and stop washing when the conductivity of washing water is 150us / cm measured by conductivity meter;

[0053] S2: Add 4.5 kg of deionized water and 15 g of ascorbic acid to the acidic dissolution tank, stir at 300 rpm, and add 1.5 kg of waste precursor Cu 0.5 Fe 0.2 Mn 0.3 , slowly add sulfuric acid, adjust the pH to 3.0, and control the temperature of the reaction system at 40°C until the waste precursor is completely dissolved.

[0054] S3: copper extraction, specifically as follows: prepare N902 copper extractant with a volume concentration of 15%; the functional sections of the extraction tank are distributed as follows: 4 extraction sections, 2 washing sections, and 4 stripping sections; copper extraction: the ratio of organic phase to aqueous phase is 1:5, the temperature of the extraction system is 40°C, and copper extraction is performed, and the copper content of the solution after copper extraction is controlled to be below 0.0002g / L.

[0055] S4: Concentrate the FeMn metal ions in the solution to 2 mol / L and add Na 2 C 2 O 4 ·H 2 O and H 2 C 2 O 4 ·2H 2 O (50:1), a light yellow precipitate was formed, and the FeMn metal ions in the solution were concentrated to 2 mol / L and dried at 65 °C under vacuum to obtain the precursor powder Mn 0.6 Fe 0.4 C 2 O 4 ·2H 2 O.

[0056] Example 5

[0057] The iron manganese oxalate precursor was prepared by coprecipitation reaction.

[0058] S1: The waste precursor Cu 0.5 Fe 0.2 Mn 0.3 Use 50℃ hot water for washing, and stop washing when the conductivity of washing water is 150us / cm measured by conductivity meter;

[0059] S2: Add 4.5 kg of deionized water and 15 g of ascorbic acid to the acidic dissolution tank, stir at 300 rpm, and add 1.5 kg of waste precursor Cu 0.5 Fe 0.2 Mn 0.3 , slowly add sulfuric acid, adjust the pH to 3.0, and control the temperature of the reaction system at 40°C until the waste precursor is completely dissolved.

[0060] S3: copper extraction, specifically as follows: prepare N902 copper extractant with a volume concentration of 15%; the functional sections of the extraction tank are distributed as follows: 4 extraction sections, 2 washing sections, and 4 stripping sections; copper extraction: the ratio of organic phase to aqueous phase is 1:5, the temperature of the extraction system is 40°C, and copper extraction is performed, and the copper content of the solution after copper extraction is controlled to be below 0.0002g / L.

[0061] S4: The FeMn metal ions in the solution are concentrated to 2 mol / L, and added to the reactor with phosphoric acid, sodium hexadecyl sulfate, and hydrogen peroxide. The pH value of the system is controlled at 3-3.5, the temperature of the reactor solution is 70°C, and the reaction is stirred at 130 rpm for 5 hours to obtain a suspension. The suspension is filtered and washed with a filter press to obtain, and then calcined at 380°C to remove free water and crystal water to obtain iron manganese phosphate precursor Mn 0.6 Fe 0.4 PO 4 .

[0062] Example 6

[0063] The iron manganese oxalate precursor was prepared by coprecipitation reaction.

[0064] S1: The waste precursor Cu 0.5 Fe 0.2 Mn 0.3 Use 50℃ hot water for washing, and stop washing when the conductivity of washing water is 150us / cm measured by conductivity meter;

[0065] S2: Add 4.5 kg of deionized water and 15 g of ascorbic acid to the acidic dissolution tank, stir at 300 rpm, and add 1.5 kg of waste precursor Cu 0.5 Fe 0.2 Mn 0.3 , slowly add sulfuric acid, adjust the pH to 3.0, and control the temperature of the reaction system at 40°C until the waste precursor is completely dissolved.

[0066] S3: copper extraction, specifically as follows: prepare N902 copper extractant with a volume concentration of 15%; the functional sections of the extraction tank are distributed as follows: 4 extraction sections, 2 washing sections, and 4 stripping sections; copper extraction: the ratio of organic phase to aqueous phase is 1:5, the temperature of the extraction system is 40°C, and copper extraction is performed, and the copper content of the solution after copper extraction is controlled to be below 0.0002g / L.

[0067] S4: The FeMn metal ions in the solution were concentrated to 2 mol / L, phosphoric acid and lithium hydroxide were dissolved in a mixed solvent consisting of water and ethylene glycol in a volume ratio of 1:2 according to Li:(Fe+Mn):P=3.03:1:P, and the solution was placed in a high-temperature and high-pressure reactor. The volume of the solution was 80% of the volume of the reactor. The solution was heated to 240°C and the reaction time was 6 hours. After natural cooling, the solution was centrifuged and washed three times, and then vacuum dried to obtain lithium iron manganese phosphate (LiFe 0.4 Mn 0.6 PO 4 )front drive. Figure 2 This is the SEM image of the waste during the preparation of the sodium ion precursor. During the precursor preparation process, due to the small solubility product of nickel salt (copper salt), iron salt and manganese salt hydroxide, the precipitation rate is fast, the solution supersaturation is high, the crystal nucleation is fast, and the colloidal precipitate is easily formed. The morphology is difficult to control. Affected by various factors such as the supersaturation of the precipitated ions in the reaction system, pH value, ammonia concentration, temperature, stirring, rate, etc., a large amount of waste precursor is inevitably generated, which cannot meet the needs of the sintering section. Figure 3 This is a SEM image of the ferrous manganese oxalate precursor prepared in Example 1. The material exhibits a polyhedral columnar structure and is evenly dispersed. The main columnar structure is composed of many thin sheets stacked together, with individual fragments scattered around the edges. Figure 4 The XRD pattern of the iron manganese phosphate precursor prepared in Example 2 matches well with PDF34-0134. Figure 5 This is a SEM image of the hydrothermal lithium iron manganese phosphate precursor prepared in Example 3, showing a nanorod morphology. The length of the nanorods ranges from 100 to 200 nm, and the width ranges from 50 to 100 nm.

[0068] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recycling waste sodium ion precursor resources, characterized in that: The following steps are involved: S1: washing and removing impurities from the waste precursors generated during the synthesis of sodium electrode precursors for multiple times; S2: Add water and reducing agent into the dissolution tank, start stirring, put in the waste precursor, and slowly add acid into the reaction system to dissolve; S3: selectively removing the Cu, Ni, Fe or Mn elements in the above solution as needed and using them as raw materials for subsequent synthetic materials; The removal of Cu adopts the copper extraction process, and the Cu ion extractant is prepared by mixing one, two or three of aldoxime, ketoxime and modifier with a diluent. The specific steps of the copper extraction process are as follows: preparing a copper extractant with a volume concentration of 10% to 20%; the functional sections of the extraction tank are distributed as follows: 4 extraction sections, 2 washing sections, and 4 stripping sections; during the copper extraction process, the ratio of the organic phase to the aqueous phase is between 1:3 and 1:8, the temperature of the extraction system is 40 to 50°C, and the copper content of the solution after copper extraction is controlled to be below 0.0005g / L; The removal of Ni adopts a nickel extraction process, and the Ni ion extractant is selected from phosphine extractants Mextral204P, Mextral507P, Cyanex272, Cyanex301 or Cyanex302; amine extractants Alamine336 or Alquit33; hydroxime extractants Mextral63H, Mextral84H, Mextral984H or Mextral860H; carboxylic acid and carboxylic acid pyridine ester extractants Ver satic10, CLX50 or 4PC, the specific steps of the nickel extraction process are as follows: prepare an extractant with a volume concentration of 30% to 40%; the functional sections of the extraction tank are distributed as follows: 12 extraction sections, 10 washing sections, and 8 stripping sections; use a 32% liquid alkali solution to saponify the organic phase, and the saponification rate is controlled at 50% to 60%; during the nickel extraction process, the organic phase to water phase ratio is between 3:1 and 5:1, the extraction temperature is between 40 and 50°C, and nickel is extracted, and the nickel content of the solution after nickel extraction is controlled to be below 0.0005g / L; S4: After the impurity-removed solution is concentrated, it reacts with a precipitant, and then solid-liquid separation is performed; The chemical formula of the waste sodium ion precursor is Ni a Cu b Fe c Mn d (OH)2, a+b+c+d=1.

2. The method for recycling waste sodium ion precursor resources according to claim 1, characterized in that: The washing in S1 is performed by multiple washing with hot pure water at 30-70° C. until the conductivity is ≤200 us / cm.

3. The method for recycling waste sodium ion precursor resources according to claim 1, characterized in that: Add 0.05~2% reducing agent according to the mass of the precursor.

4. The method for recycling waste sodium ion precursor resources according to claim 1, characterized in that: The reducing agent includes one of hydrazine hydrate, ascorbic acid, pyrosulfite and sulfur dioxide.

5. The method for recycling waste sodium ion precursor resources according to claim 1, characterized in that: The acid in S2 is one or a mixture of sulfuric acid, nitric acid, phosphoric acid, hydrochloric acid, perchloric acid, hydrobromic acid, hydroiodic acid, citric acid, oxalic acid, formic acid, etc.

6. The method for recycling waste sodium ion precursor resources according to claim 1, characterized in that: The temperature of the reaction system in S2 is 30-60° C., and the pH is 2-5.

7. The method for recycling waste sodium ion precursor resources according to claim 1, characterized in that: The Cu ion extractant was N902 copper extractant, and the Ni ion extractant was Cyanex272 extractant.

Citation Information

Patent Citations

  • Copper-iron-manganese / nickel layered oxide precursor for sodium ion battery and preparation method and use thereof

    CN109037671A

  • Method for comprehensively extracting metal from waste lithium ion battery

    CN111041218A

  • Method for preparing nickel-manganese-iron ternary precursor and iron phosphate by recycling waste batteries

    CN116947118A

  • Recovery method for valuable metals in waste nickel-cobalt-manganese ternary lithium batteries

    WO2020220559A1